Chiral self-polymerized microporous polymer fluorescent probe and preparation method and fluorescent recognition application thereof

By synthesizing a chiral, soluble, chain-like self-polymerizing microporous polymer based on the structural unit of 3,3,3′,3′-tetramethyl-1,1′-spirodiindene-7,7′-diol, the problem of complex and expensive preparation of existing chiral PIMs materials has been solved, and efficient small molecule enantiomeric fluorescence recognition with readily available raw materials and simple operation has been achieved.

CN118930771AActive Publication Date: 2024-11-12SHANDONG UNIV +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410918004.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12
Estimated Expiration
2044-07-10

Smart Images

  • Figure CN118930771A_ABST
    Figure CN118930771A_ABST
Patent Text Reader

Abstract

The invention relates to a chiral self-polymerized microporous polymer fluorescent probe as well as a preparation method and fluorescent recognition application thereof. The chiral self-polymerized microporous polymer fluorescent probe comprises a chiral soluble chain-shaped self-polymerized microporous polymer shown in the following formula I or an enantiomer of the polymer. The chiral spirodiindenyl microporous polymer has specific recognition on a small molecule enantiomer; especially, the fluorescent probe has specific fluorescence enhancement performance on an enantiomer of phenylalanine, and can be used for molecular enantiomer identification. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a chiral self-polymerizing microporous polymer fluorescent probe and a preparation method and fluorescent identification application thereof, belonging to the technical field of organic polymer materials and molecular probes. Background Art

[0002] Chirality is a widespread phenomenon in nature, and this property profoundly affects the properties and functions of various substances. The construction of precise chiral systems and the development of efficient enantiomer differentiation technologies are regarded as the core driving force in many fields such as pharmaceutical research and development, information technology, advanced materials science, and computational science, but they are still facing many technical bottlenecks and challenges. Among the many chiral recognition strategies, chromatographic separation, electrochemical analysis, and spectral analysis techniques occupy a pivotal position, especially their outstanding contributions to the identification of chiral molecular enantiomers cannot be ignored. However, the popularization and application of traditional chromatographic technology is significantly restricted due to its limitations such as high cost, complex pretreatment process, and time-consuming. In contrast, fluorescence spectroscopy, as a rising star in the field of chiral recognition, is gradually winning wide recognition and attention from the scientific research community with its significant advantages such as rapid response, high selectivity, and low detection threshold.

[0003] In order to further improve the sensitivity and selectivity of chiral recognition, the design and synthesis of high-performance chiral fluorescent probes has become a research hotspot. At present, a variety of chiral fluorescent recognition materials have been successfully developed, including but not limited to chiral ionic liquids, chiral covalent organic frameworks (COFs), chiral metal organic frameworks (MOFs), porous organic cages and natural proteins. It is particularly worth mentioning that self-supporting microporous materials, with their ultra-high specific surface area, excellent structural stability and outstanding functionalization potential, are expected to play a more important role in the innovation of chiral recognition technology and show great application prospects.

[0004] As a unique type of chain polymer, the characteristic feature of intrinsic microporous materials (PIMs) is their rigid main chain structure. This rigidity limits the free rotation of the molecular chain, thereby preventing the effective stacking between chains and naturally forming a continuous microporous network inside the material. This type of material not only exhibits excellent solubility and film-forming ability, but also attracts widespread attention in cutting-edge fields such as gas separation and sensing technology. However, in the family of PIMs, the research on chiral PIMs is just getting started. The literature Angew.Chem.Int.Ed.2015,54,11214-11218 reported a chiral PIM-1 prepared by condensation of chiral spirobiindene TTSBI and 2,3,5,6-tetrafluoroterephthalonitrile, which was used for chiral membrane separation of small molecules; the literature Angew.Chem.Int.Ed.2021,60,12781-12785 reported a chiral porous polymer FTPI based on triptycene structure, which was also used for small molecule membrane separation; the literature Macromolecules 2021,54,11180-11186 reported a chiral CCS-PIM with a [5,5,6]-cyclohexane spirobiindene unit, which was found to have circularly polarized luminescence characteristics; despite this, PIMs materials with backbone chirality are still very rare, and research on the use of PIMs as fluorescent sensing materials for enantiomeric recognition of small molecules has not been reported. At the same time, the preparation process of the reported chiral PIMs materials is complicated, the reagents used are expensive, and it is difficult to produce on a large scale. Therefore, exploring and developing new backbone chiral PIMs materials not only has far-reaching academic value, but also has important practical significance, and is expected to bring technological innovation and breakthroughs to the field of chiral recognition.

[0005] After searching, there are currently no literature reports on chiral PIMs materials based on 3,3,3′,3′-tetramethyl-1,1′-spirobiindene-7,7′-diol structural units, and small molecule enantiomer recognition using PIMs as fluorescent probes. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a chiral self-polymerizing microporous polymer fluorescent probe and a preparation method and fluorescence recognition application thereof.

[0007] The present invention is achieved through the following technical solutions:

[0008] A chiral soluble chain-like self-polymerizing microporous polymer or an enantiomer of the polymer having the following formula I:

[0009]

[0010] Wherein R1, R2, R3, and R4 are each independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, fluorine, chlorine, bromine, iodine, hydroxyl, or mercapto, and n is a positive integer.

[0011] More preferably, R1, R2, R3, and R4 are each hydrogen, and n is a positive integer ≥1.

[0012] Preferably according to the present invention, in the structure shown in Formula I, the spirobiindene unit or its enantiomer structure is shown in Formula II below:

[0013]

[0014] According to the present invention, preferably, the spirobiindene unit or its enantiomer is prepared by the following method:

[0015] Bisphenol A is stirred in an acid solution to undergo cracking and rearrangement to generate a racemic diphenol spirobiindene compound 1; the racemic diphenol spirobiindene compound 1 undergoes an esterification reaction in the presence of an alkaline catalyst and an optically pure chiral auxiliary reagent to generate a diastereomeric mixture RL-2 and SL-2; then it is recrystallized at low temperature to precipitate RL-2; finally, the auxiliary group is hydrolyzed to obtain an optically pure spirobiindene unit.

[0016] According to the preferred embodiment of the present invention, the acid solution is methanesulfonic acid;

[0017] According to the present invention, preferably, the base catalyst is 4-dimethylaminopyridine (DMAP);

[0018] According to the present invention, the chiral auxiliary reagent is preferably L-menthylformyl chloride;

[0019] Preferably, according to the present invention, the mass volume ratio of bisphenol A to acid solution is (2-6): (15-25), unit, g / mL, the cracking and rearrangement temperature is room temperature, and the reaction time is 1-3 days.

[0020] Preferably, according to the present invention, the mass ratio of the racemic diphenol spirobiindene compound 1 to the base catalyst is (450-550):(10-20).

[0021] Preferably according to the present invention, the mass volume ratio of the racemic diphenol spirobiindene compound 1 to the chiral auxiliary reagent is (450-550):(0.5-2), unit, g / mL.

[0022] Preferably according to the present invention, the esterification reaction is carried out in dichloromethane, and triethylamine is added at the same time, and the mass volume ratio of the racemic diphenol spirobiindene compound 1 to dichloromethane is (450-550): (2-10), unit, g / mL, and the mass volume ratio of the racemic diphenol spirobiindene compound 1 to triethylamine is (450-550): (0.5-2), unit, g / mL.

[0023] According to the preferred embodiment of the present invention, the crystallization temperature is -15 to -20°C.

[0024] According to a preferred embodiment of the present invention, the auxiliary group is hydrolyzed by refluxing in an ethanol solution of potassium hydroxide.

[0025] The reaction route of the spirobiindene unit or its enantiomer is shown in III below:

[0026]

[0027] The present invention also provides a method for preparing the self-polymerized microporous polymer. The method comprises the following steps:

[0028] The optically pure compound monomer II and indigo carmine are mixed, anhydrous dichloromethane is added under ice-water bath cooling, and trifluoroacetic acid is added dropwise, and the mixture is stirred for half an hour until the solution is evenly mixed. Trifluoromethanesulfonic acid is then added dropwise, and the mixture is stirred at room temperature until the solution becomes viscous. The reaction solution is added to a methanol / water mixed solution to form a flocculent precipitate, and ammonia water is added to remove excess acid. The filter cake is filtered to obtain a target polymer brown solid product after dissolution-precipitation.

[0029] The specific surface area of ​​the self-polymerized microporous polymer prepared by the present invention is 50m 2 / g-1000m 2 / g.

[0030] Preferably according to the present invention, the molar ratio of the optically pure compound monomer II to isatin is 1:1.

[0031] Preferably according to the present invention, the molar ratio of the monomer to the total volume of anhydrous dichloromethane, trifluoroacetic acid and trifluoromethanesulfonic acid is 0.01:(10-35), unit, mol / mL.

[0032] Preferably according to the present invention, the volume ratio of anhydrous dichloromethane, trifluoroacetic acid and trifluoromethanesulfonic acid is 1:1:1.

[0033] The reaction route of chiral spirobiindene self-microporous polymer is shown in Formula IV below:

[0034]

[0035] wherein R1, R2, R3, and R4 are each independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, fluorine, chlorine, bromine, iodine, hydroxyl, or mercapto; and n is a positive integer.

[0036] The chiral soluble chain-like self-polymerized microporous polymer as shown in formula I is used for molecular fluorescence recognition.

[0037] Preferably, the molecular fluorescence identification method is as follows:

[0038] The chiral soluble chain self-polymerizing microporous polymer shown in formula I is dissolved in methanol to obtain a mixed solution a, and the mixed solution a is added to a quartz cuvette, and the ultraviolet absorption spectrum at the emission wavelength and the fluorescence emission spectrum at the excitation wavelength are measured as background values; the chiral soluble chain self-polymerizing microporous polymer shown in formula I and a methanol solution of a small molecule to be analyzed are accurately prepared to obtain a mixed solution b, and the mixed solution b is added to a quartz cuvette, and the fluorescence luminescence curve of the mixed solution at the excitation wavelength is measured.

[0039] Preferably, the concentration of the self-polymerized microporous polymer in the mixed solution a and the mixed solution b is 1×10 -5 mol / L.

[0040] Preferably, the concentration of the small molecule to be analyzed in the mixed solution b is 5×10 -5 mol / L, the small molecule to be analyzed is D-phenylalanine or D-binaphthol.

[0041] Preferably, the ultraviolet absorption wavelength is 400nm;

[0042] Preferably, the excitation wavelength is 270 nm;

[0043] Preferably, the fluorescence emission wavelength is 290 to 800 nm.

[0044] The technical features and advantages of the present invention are as follows:

[0045] 1. The self-microporous polymer of the present invention is optically pure.

[0046] 2. The self-microporous polymer of the present invention is soluble in organic solvents such as methanol and tetrahydrofuran.

[0047] 3. The soluble self-microporous polymer methanol solution of the present invention has specific fluorescence enhancement for D-phenylalanine, which is significantly higher than that of L-phenylalanine, and can meet the actual requirements for the recognition of phenylalanine enantiomers.

[0048] 4. The raw materials are easily available, the operation is simple, and it is convenient for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 is the H NMR spectrum of the chiral compound II spirobiindene monomer of Example 1;

[0050] Figure 2 is the NMR carbon spectrum of the chiral spirobiindene self-microporous polymer prepared in Example 1;

[0051] Figure 3 is the nitrogen physical adsorption isotherm of the chiral spirobiindene self-microporous polymer obtained in Example 1,

[0052] Figure 4The following are the H NMR spectra, UV absorption and fluorescence spectra of the chiral spirobiindene self-microporous polymer prepared in Example 1.

[0053] Figure 5 The chiral spirobiindene self-microporous polymer prepared in Example 1 is selectively used for recognizing a series of small molecule enantiomers. DETAILED DESCRIPTION

[0054] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0055] Example 1

[0056] Preparation method of self-polymerized microporous polymer:

[0057] (1) Preparation of polymer monomers

[0058]

[0059] The preparation steps of compound 1 are as follows: 4 g of bisphenol A is added to 18 mL of methanesulfonic acid, stirred at room temperature for 3 days, and then crushed ice is added until solid no longer precipitates. The reaction system is filtered, and the filter cake is washed with hot water and saturated sodium bicarbonate until neutral to obtain a crude product of racemic diphenol spirobiindene compound 1. The obtained crude product solid is dissolved in ethanol, and recrystallized and filtered to obtain a white flocculent solid (3,3,3′,3′-tetramethyl-1,1′-spirobiindene-7,7′-diol (6,6′-TMSOL)), with a yield of 81.2%.

[0060] Nuclear magnetic resonance 1H NMR (600 MHz, DMSO-d6) δ8.97 (d, J=1.2 Hz, 1H), 6.97 (d, J=8.2 Hz, 2H), 6.57 (ddd, J=8.2, 2.4, 0.8 Hz, 2H), 6.07 (d, J=2.3 Hz, 2H), 2.23 (d, J=12.9 Hz, 2H), 2.07 (d, J=12.9 Hz, 2H), 1.29 (s, 6H), 1.22 (s, 6H).

[0061]

[0062] The preparation steps of optically pure compound RL-2 are as follows:

[0063] a. Add 500 mg of compound 1 and 16.3 mg of 4-dimethylaminopyridine (DMAP) into a round-bottom flask, add 4 mL of dichloromethane, 0.75 mL of triethylamine and 0.75 mL of L-menthol acid methyl chloride in sequence, and stir at room temperature for 1 h under N2 atmosphere. Then wash with 1 mol / L hydrochloric acid and saturated sodium chloride, extract with ethyl acetate, dry the oil phase with anhydrous sodium sulfate after separation, separate with silica gel column (ethyl acetate: petroleum ether 1:100) and dry with rotary evaporation to obtain a mixture of RL-2 and SL-2.

[0064] b. The crude mixture of RL-2 and SL-2 was dissolved in n-hexane, concentrated to near saturation, and placed in a refrigerator overnight to precipitate crystals. The mother liquor was carefully removed with a pipette, and the crystals were washed twice with cold n-hexane and dried to obtain white crystals of RL-2, with a yield of 31.4%. The purity of the product was analyzed by HPLC with a C18 column, the mobile phase was methanol: water = 90:10, and the retention time was: RT (RL-2) = 37.5 min, RT (SL-2) = 41.1 min.

[0065] RL-2 NMR: 1H NMR(600MHz,Chloroform-d)δ7.14(d,J=8.3Hz,2H),7.03(dd,J=8.3,2.3Hz,2H),6.61(d ,J=2.2Hz,2H),4.55(td,J=10.9,4.5Hz,2H),2.36(d,J=13.1Hz,2H),2.27(d,J=13.1Hz, 2H),2.13(dq,J=12.0,4.9,4.3Hz,2H),2.06~1.94(m,2H),1.68(ddt,J=13.0,5.3,2.8Hz ,4H),1.51~1.27(m,16H),1.13~1.00(m,4H),0.93~0.87(m,14H),0.79(d,J=7.0Hz,6H).

[0066]

[0067] The preparation steps of optically pure polymer monomer R-1 are as follows: dissolve RL-2 solid in ethanol, add potassium hydroxide, heat under reflux for 2 hours, and then concentrate in vacuo. The resulting residual liquid is extracted with dichloromethane, and the organic phase is washed with 1 mol / L hydrochloric acid and saturated sodium chloride solution, dried over anhydrous sodium sulfate, and rotary evaporated to obtain white flocculent crystals ((R)-3,3,3′,3′-tetramethyl-1,1′-spirobiindene-7,7′-diol, (R)-6,6'-TMSOL) with a yield of 80.4%.

[0068] The NMR results are consistent with the racemic diphenol spirobiindene compound 1: 1H NMR (600MHz, DMSO-d6) δ8.97 (d, J = 1.2Hz, 1H), 6.97 (d, J = 8.2Hz, 2H), 6.57 (ddd, J = 8.2, 2.4, 0.8Hz, 2H), 6.07 (d, J = 2.3Hz, 2H), 2.23 (d, J = 12.9Hz, 2H), 2.07 (d, J = 12.9Hz, 2H), 1.29 (s, 6H), 1.22 (s, 6H). The NMR spectrum of the spirobiindene unit is shown in Figure 1 shown.

[0069] (2) Preparation of Chiral Spirobiindene Microporous Polymer 3:

[0070]

[0071] The optically pure monomer R-1 (6,6'-TMSOL, 0.01 mol) obtained in step (1) and indigo carmine (0.01 mol) were mixed in a round-bottom flask. Under ice-water bath cooling conditions, 3 ml of anhydrous dichloromethane was added, and 3 ml of trifluoroacetic acid was added dropwise. The mixture was stirred for half an hour until the solution was evenly mixed. Then 3 ml of trifluoromethanesulfonic acid was added dropwise. The mixture was stirred at room temperature until the solution became viscous. The reaction solution was added to a mixed solution of methanol: water = 1:1 to form a flocculent precipitate. A small amount of ammonia water was added to remove excess acid, and the filter cake was filtered. The obtained solid was dissolved in tetrahydrofuran, and the mixed solution of methanol: water = 1:1 was poured again to precipitate the polymer. The mixture was vacuum dried at 120°C for 12 hours to obtain a dark red solid with a yield of 87.7%.

[0072] 1H NMR (600MHz, DMSO-d6) δ10.92 (s, 1H), 10.01 (s, 1H), 9.04 (d, J = 77.0Hz, 1H), 7.53~5.59 (m, 8H), 2.09 (s, 4H), 1.67~0.5 (m, 12H).

[0073] The NMR carbon spectrum, physical adsorption isotherm, UV and fluorescence spectra of polymer 3 are shown in Figure 2 , Figure 3 , Figure 4 As shown, it is demonstrated that the present invention successfully prepared chiral spirobiindene self-microporous polymer.

[0074] (3) Fluorescence selectivity of chiral polymers for phenylalanine enantiomers:

[0075] 1) Dissolve chiral polymer 3 in methanol and prepare 2×10 -5mol / L solution A, take 2 ml of solution A and mix with 2 ml of methanol, add into a quartz cuvette, measure the fluorescence emission spectrum under the excitation wavelength of 271 nm, and select the fluorescence intensity at the wavelength of 366 nm as I0;

[0076] 2) Prepare D-phenylalanine at a concentration of 1×10 -4 2 ml of 1 mol / L methanol solution was taken and mixed with 2 ml of solution A, and then added into a quartz cuvette. The fluorescence emission spectrum was measured at an excitation wavelength of 271 nm, and the fluorescence intensity at a wavelength of 366 nm was recorded as I d .

[0077] 3) Accurately configure the concentration of L-phenylalanine to 1×10 -4 2 ml of 1 mol / L methanol solution was taken and mixed with 2 ml of solution A, and then added into a quartz cuvette. The fluorescence emission spectrum was measured at an excitation wavelength of 271 nm, and the fluorescence intensity at a wavelength of 366 nm was recorded as I l .

[0078] The enantiomeric fluorescence selectivity is S = |(I l -I0) / (I d -I0)|.

[0079] Example 2

[0080] Preparation method of self-polymerized microporous polymer

[0081] (1) The polymer monomer was prepared according to step (1) of Example 1;

[0082] (2) Preparation of chiral soluble chain-like self-polymerized microporous polymers:

[0083] Under the protection of nitrogen atmosphere, optically pure monomer R-1 (6,6'-TMSOL, 0.05 mol) and indigo carmine (0.015 mol) were mixed in a round-bottom flask. Under ice-water bath cooling, 10 ml of anhydrous dichloromethane was added, and 10 ml of trifluoroacetic acid was added dropwise. Stirring was continued for half an hour until the solution was evenly mixed. Then 10 ml of trifluoromethanesulfonic acid was added dropwise. Stirring was continued at room temperature until the solution became viscous. The reaction solution was added to a mixed solution of methanol: water = 1:1 to form a flocculent precipitate. A small amount of ammonia water was added to remove the excess acid, and the filter cake was filtered. The obtained solid was dissolved in tetrahydrofuran, and the mixed solution of methanol: water = 1:1 was poured again to precipitate the polymer. Vacuum drying was carried out at 120°C for 12 hours to obtain a dark red solid with a yield of 90.1%.

[0084] (3) Fluorescence selectivity test of chiral polymers for binaphthol enantiomers:

[0085] 1) Dissolve chiral polymer 3 in methanol and prepare 2×10-5 mol / L solution A, take 2 ml of solution A and mix it with 2 ml of methanol, add it into a quartz cuvette, measure the fluorescence emission spectrum under the excitation wavelength of 271 nm, and select the fluorescence intensity at the wavelength of 366 nm as I0.

[0086] 2) Accurately prepare the concentration of D-binaphthol to 1×10 -4 2 ml of mol / L methanol solution was taken and mixed with 2 ml of solution A, added into a quartz cuvette, and the fluorescence emission spectrum was measured at an excitation wavelength of 271 nm. The fluorescence intensity at a wavelength of 366 nm was recorded as I d .

[0087] 3) Accurately prepare the concentration of L-binaphthol to 1×10 -4 2 ml of mol / L methanol solution was taken and mixed with 2 ml of solution A, added into a quartz cuvette, and the fluorescence emission spectrum was measured at an excitation wavelength of 271 nm. The fluorescence intensity at a wavelength of 366 nm was recorded as I l .

[0088] The enantiomeric fluorescence selectivity is S = |(I l -I0) / (I d -I0)|.

Claims

1. A chiral soluble chain-like self-polymerizing microporous polymer or an enantiomer of the polymer having the following formula I: Wherein R1, R2, R3, and R4 are each independently hydrogen, alkyl, cycloalkyl, alkoxy, aryl, fluorine, chlorine, bromine, iodine, hydroxyl or mercapto, and n is a positive integer. Preferably, R1, R2, R3, and R4 are each hydrogen, and n is a positive integer ≥1.

2. The chiral soluble chain-like self-polymerizing microporous polymer or the enantiomer of the polymer according to claim 1, characterized in that: In the structure shown in Formula I, the spirobiindene unit or its enantiomer structure is shown in Formula II below:

3. The chiral soluble chain-like self-polymerizing microporous polymer or the enantiomer of the polymer according to claim 1, characterized in that: The spirobiindene unit or its enantiomer is prepared as follows: Bisphenol A is stirred in an acid solution to undergo cracking and rearrangement to generate a racemic diphenol spirobiindene compound 1; the racemic diphenol spirobiindene compound 1 undergoes an esterification reaction in the presence of an alkaline catalyst and an optically pure chiral auxiliary reagent to generate a diastereomeric mixture RL-2 and SL-2; then it is recrystallized at low temperature to precipitate RL-2; finally, the auxiliary group is hydrolyzed to obtain an optically pure spirobiindene unit.

4. The chiral soluble chain-like self-polymerizing microporous polymer or the enantiomer of the polymer according to claim 3, characterized in that: The acid solution is methanesulfonic acid; the base catalyst is 4-dimethylaminopyridine (DMAP); and the chiral auxiliary reagent is L-menthylformyl chloride.

5. The chiral soluble chain-like self-polymerizing microporous polymer or the enantiomer of the polymer according to claim 3, characterized in that: The mass volume ratio of bisphenol A to the acid solution is (2-6): (15-25), unit, g / mL, the cracking rearrangement temperature is room temperature, the reaction time is 1-3 days, the mass ratio of the racemic diphenol spirobiindene compound 1 to the base catalyst is (450-550): (10-20), and the mass volume ratio of the racemic diphenol spirobiindene compound 1 to the chiral auxiliary reagent is (450-550): (0.5-2), unit, g / mL.

6. The chiral soluble chain-like self-polymerizing microporous polymer or the enantiomer of the polymer according to claim 3, characterized in that: The esterification reaction is carried out in dichloromethane, and triethylamine is added at the same time. The mass volume ratio of the racemic diphenol spirobiindene compound 1 to dichloromethane is (450-550):(2-10), unit, g / mL, and the mass volume ratio of the racemic diphenol spirobiindene compound 1 to triethylamine is (450-550):(0.5-2), unit, g / mL. The crystallization temperature is -15 to -20°C, and the auxiliary group is hydrolyzed by refluxing in an ethanol solution of potassium hydroxide.

7. A method for preparing the chiral soluble chain-like self-polymerizing microporous polymer or the enantiomer of the polymer according to claim 1, comprising the following steps: The optically pure compound monomer II and indigo carmine are mixed, anhydrous dichloromethane is added under ice-water bath cooling, and trifluoroacetic acid is added dropwise, and the mixture is stirred for half an hour until the solution is evenly mixed. Trifluoromethanesulfonic acid is then added dropwise, and the mixture is stirred at room temperature until the solution becomes viscous. The reaction solution is added to a methanol / water mixed solution to form a flocculent precipitate, and ammonia water is added to remove excess acid. The filter cake is filtered to obtain a target polymer brown solid product after dissolution-precipitation.

8. The preparation method according to claim 7, characterized in that: The molar ratio of optically pure compound monomer II to indigo is 1:1, the molar amount of the monomer to the total volume ratio of anhydrous dichloromethane, trifluoroacetic acid and trifluoromethanesulfonic acid is 0.01:(10-35), unit, mol / mL, and the volume ratio of anhydrous dichloromethane, trifluoroacetic acid and trifluoromethanesulfonic acid is 1:1:

1.

9. Use of the chiral soluble chain-like self-polymerizing microporous polymer or the enantiomer of the polymer as claimed in claim 1 for molecular fluorescence recognition.

10. The use according to claim 9, characterized in that: The molecular fluorescence identification method is as follows: The chiral soluble chain-like self-polymerized microporous polymer shown in Formula I is dissolved in methanol to obtain a mixed solution a, and the mixed solution a is added to a quartz cuvette, and the ultraviolet absorption spectrum at the emission wavelength and the fluorescence emission spectrum at the excitation wavelength are measured as background values; the chiral soluble chain-like self-polymerized microporous polymer shown in Formula I and a methanol solution of a small molecule to be analyzed are accurately prepared to obtain a mixed solution b, and the mixed solution b is added to a quartz cuvette, and the fluorescence emission curve of the mixed solution at the excitation wavelength is measured; The concentration of the self-polymerized microporous polymer in the mixed solution a and the mixed solution b is 1×10 -5 mol / L; The concentration of the small molecule to be analyzed in the mixed solution b is 5×10 -5 mol / L, the small molecule to be analyzed is D-phenylalanine or D-binaphthol; The ultraviolet absorption wavelength is 400nm, the excitation wavelength is 270nm, and the fluorescence emission wavelength is 290~800nm.

Citation Information

Patent Citations

  • Synthesis of PIM (polymer of intrinsic microporosity), and preparation method and application of PIM membrane

    CN107213807A

  • Isatin copolymers having intrinsic microporosity

    CN107636051A

  • Chiral self-contained microporous polymer as well as preparation method and application thereof

    CN112646170A

  • Chiral recognition polymer and its use to separate enantiomers

    US6265615B1