Lignin modified urea-formaldehyde resin for ENF-grade artificial board as well as preparation method and application of lignin modified urea-formaldehyde resin
By developing a method for preparing lignin-modified urea-formaldehyde resin, the problem of formaldehyde release in ENF-grade engineered wood products has been solved, enabling the production of low-cost, high-environmentally friendly, and high-mechanical-performance ENF-grade engineered wood products that meet the formaldehyde emission limits of the new national standards.
Patent Information
- Application Number
- CN202411226335.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
Existing urea-formaldehyde resin-based engineered wood products have formaldehyde release issues during manufacturing and use, making it difficult to simultaneously meet the requirements for high environmental protection standards and mechanical properties. In particular, in the production of ENF-grade engineered wood products, traditional adhesive technologies are unable to meet the formaldehyde release limits required by the new national standards.
A method for preparing lignin-modified urea-formaldehyde resin was adopted. By adding urea in multiple stages and controlling the reaction conditions, combined with polyvinyl alcohol and triazine nitrogen-containing heterocyclic organic compounds, and adjusting the pH value, an ENF-grade modified urea-formaldehyde resin for engineered wood products was prepared, which reduced the release of free formaldehyde and improved the bonding strength and mechanical properties.
It has achieved low-cost production of ENF-grade engineered wood panels with good stability, reduced formaldehyde emissions, and improved bonding strength and immersion peel strength, meeting the environmental protection requirements of the new national standards.
Smart Images

Figure BDA0005024680720000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of urea-formaldehyde resin production, in particular to the field of IPC C08G12 / 40, and more specifically to a lignin-modified urea-formaldehyde resin for ENF-grade artificial panels, and a preparation method and application thereof. Background Art
[0002] Artificial boards are made of natural wood and adhesives. Natural wood is flammable and also poses a potential threat to people's lives and property. In the manufacturing process of artificial boards, the adhesive resin is cured and adhered to the surface of the wood. While playing a bonding role, it also isolates oxygen to a certain extent and slows down the combustion process. Therefore, formaldehyde-free adhesives that have both excellent bonding properties and excellent flame retardant properties can undoubtedly significantly improve the safety of artificial board products. With the new national standards "Classification of Formaldehyde Emissions of Artificial Boards and Their Products" (GB / T39600-2021) and "Guidelines for Indoor Load Limits of Artificial Boards Based on Limit Formaldehyde Emissions" (GB / T39598-2021) officially implemented on October 1, 2021, traditional artificial board adhesive technology urgently needs to be upgraded to meet higher indoor board formaldehyde emission limit standards, especially the use of traditional aldehyde series resins to produce ENF grade (≤0.025mg / m 3 ) Artificial boards are an urgent need for the current artificial board industry at home and abroad. Among them, artificial boards produced with urea-formaldehyde resin have the problem of formaldehyde release during the manufacturing and use process. The quality of boards on the market is currently different, and very few of them can meet both environmental protection grades and mechanical properties. Summary of the invention
[0003] The first aspect of the present invention provides a lignin-modified urea-formaldehyde resin for ENF-grade artificial boards, the components of which include formaldehyde, urea, triazine-type nitrogen-containing heterocyclic organic compounds, alkali solution, acid solution, lignin-type polymer compounds, polyvinyl alcohol, additives and water.
[0004] Preferably, in parts by weight, the lignin-modified urea-formaldehyde resin component includes: 8000-12000 parts of formaldehyde, 7500-10000 parts of urea, 1000-1500 parts of triazine-type nitrogen-containing heterocyclic organic compounds, 30-50 parts of alkali solution, 25-35 parts of acid solution, 200-500 parts of lignin-type polymer compounds, 50-100 parts of polyvinyl alcohol, 5000-13000 parts of additives, and 500-2000 parts of water.
[0005] The ratio of the polyvinyl alcohol to the lignin polymer compound is 1:(8-20).
[0006] Preferably, the ratio of the polyvinyl alcohol to the lignin-based polymer compound is 1:(8-15).
[0007] The triazine nitrogen-containing heterocyclic organic compound includes at least one of melamine, triallyl cyanurate, cyanuric chloride and trichloromelamine.
[0008] The average polymerization degree of the polyvinyl alcohol is 1800-3000.
[0009] Preferably, the average degree of polymerization of the polyvinyl alcohol is 2000-2800.
[0010] The auxiliary agent includes a first auxiliary agent, a second auxiliary agent and a third auxiliary agent, the first auxiliary agent includes an ammonium salt, the second auxiliary agent includes at least one of a sodium salt and a magnesium salt, and the third auxiliary agent includes an aqueous solution of a sodium salt.
[0011] Preferably, the ammonium salt is selected from at least one of ammonium bicarbonate, ammonium phosphate, ammonium nitrate, ammonium chloride and ammonium sulfate.
[0012] The alkali solution includes an aqueous solution of at least one of sodium hydroxide, potassium hydroxide, magnesium hydroxide and ammonia water.
[0013] The acid solution includes a solution of at least one of formic acid, acetic acid, sulfuric acid, hydrochloric acid, and phosphoric acid.
[0014] The lignin-based polymer compound includes at least one of lignin, lignin sulfonate, and lignin carboxylate.
[0015] The second aspect of the present invention provides a method for preparing a lignin-modified urea-formaldehyde resin for an ENF-grade wood-based panel, comprising the following steps:
[0016] S1, adding formaldehyde, polyvinyl alcohol, lignin polymer compound, and water, adding alkali solution to adjust the pH value to 7.2-8, adding 20-40wt% of urea, 20-40wt% of the first auxiliary agent, the third auxiliary agent, the second auxiliary agent, and 35-50wt% of the triazine nitrogen-containing heterocyclic organic compound to react;
[0017] S2, cooling to 85-90°C, adding acid to adjust the pH value to 6.0-6.5, reacting for 2-10 minutes, then adding acid to adjust the pH value to 5.0-5.5, adding 15-25wt% of a total amount of a triazine nitrogen-containing heterocyclic organic compound, and carrying out a heat-insulating reaction;
[0018] S3, adding alkali solution to adjust the pH value to 5.5-6.2, adding 10-20wt% of urea in total, adding alkali solution to adjust the pH value to 6.0-6.5, adding the remaining triazine nitrogen-containing heterocyclic organic compound and 10-20wt% of urea in total;
[0019] S4, add alkali solution to adjust the pH value to 7.0-7.5, add the remaining first auxiliary agent, add a total of 15-30wt% urea, cool to 65-75°C, add alkali solution to adjust the pH value to 7.5-8.0, add the remaining urea, cool to 38-45°C, and obtain.
[0020] The reaction temperature in step S1 is 88-94° C., and the reaction time is 25-35 min.
[0021] The present application has found that adding urea in multiple batches can improve the mechanical properties of the modified urea-formaldehyde resin and reduce the free formaldehyde content. The first urea in step S1 is mainly used to synthesize the resin body of the urea-formaldehyde resin. The amount of this part determines the bonding strength of the resin. If the amount of formaldehyde added in S1 is too high, the bonding strength of the resin is high and the curing speed is fast, but the free formaldehyde release is significantly increased, and the instability of the resin is also very obvious; when the amount of formaldehyde added is low, the bonding strength of the resin is insufficient and the curing time will also be extended. The reason for adding the remaining urea in three batches in step S3 is to allow it to fully react with the free formaldehyde in the system under specific weak alkaline conditions, and to control the amount of urea added in each batch to minimize the free formaldehyde release without affecting the bonding strength of the resin.
[0022] Preferably, the reaction temperature in step S1 is 90-94° C., and the reaction time is 25-35 min.
[0023] The product of the heat preservation reaction in step S2 has a viscosity of 12-15s at 30°C for 4 cups.
[0024] Preferably, the product of the heat preservation reaction in step S2 has a coating viscosity of 13-14s at 30°C.
[0025] The product obtained in step S3 has a coating viscosity of 14-17s at 30°C.
[0026] Preferably, the product obtained in step S3 has a coating viscosity of 15-16s at 30°C.
[0027] The third aspect of the present invention provides an application of a lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels, characterized in that it is applied to at least one of solid wood panels, ecological panels, and blockboards.
[0028] Beneficial effects:
[0029] 1. The modified urea-formaldehyde resin prepared in this application is suitable for the production of ENF-grade artificial boards, with low cost and good stability.
[0030] 2. The ratio of polyvinyl alcohol to lignin polymer compound is 1:(8-20), which can be applied to artificial boards to reduce the formaldehyde emission in the artificial boards and make them reach ENF level.
[0031] 3. The reaction temperature in step S1 is 88-94°C and the reaction time is 25-35 minutes, which can improve the type II immersion peel strength.
[0032] 4. The present application adds urea in multiple times, which can improve the mechanical properties of the modified urea-formaldehyde resin and reduce the free formaldehyde content.
[0033] 5. The average polymerization degree of the polyvinyl alcohol is 1800-3000, and its application in artificial boards can simultaneously improve the bonding strength and immersion peeling. DETAILED DESCRIPTION
[0034] Example 1
[0035] The invention discloses a lignin-modified urea-formaldehyde resin for ENF-grade artificial board, wherein the raw materials for preparing the urea-formaldehyde resin are: formaldehyde (37 wt% aqueous solution), urea, triazine nitrogen-containing heterocyclic organic compound (melamine), alkali solution (sodium hydroxide aqueous solution, concentration of 32 wt%), acid solution (formic acid aqueous solution, concentration of 20 wt%), lignin, polyvinyl alcohol (Taiwan Changchun, BP-26), additives and water.
[0036] The auxiliary agent comprises a first auxiliary agent, a second auxiliary agent and a third auxiliary agent, wherein the first auxiliary agent is ammonium bicarbonate, the second auxiliary agent is sodium sulfate, and the third auxiliary agent comprises a 20 wt % sodium chloride aqueous solution.
[0037] A method for preparing lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels (raw materials are calculated by weight), comprising the following steps:
[0038] S1: Add 8000 parts of 37wt% formaldehyde, 50 parts of polyvinyl alcohol, 200 parts of lignin, and 1000 parts of water into a reactor, add alkali solution to adjust the pH value to 7.5, add 3000 parts of urea, 1000 parts of the first auxiliary agent, 5000 parts of the third auxiliary agent, 50 parts of the second auxiliary agent, and 250 parts of the triazine nitrogen-containing heterocyclic organic compound, and then heat to 92°C and keep warm for 30 minutes;
[0039] S2 is cooled to 88°C, and acid is added twice. The first time acid is added, the pH value is adjusted to 6.1, and the reaction is performed for 4 minutes. The second time acid is added, the pH value is adjusted to 5.1, and 100 parts of triazine nitrogen-containing heterocyclic organic compounds are added. The reaction is kept warm until the viscosity at 30°C is (coating-4 cups) 13-14s;
[0040] S3 adds alkali solution to adjust the pH value to 5.8, adds 1000 parts of urea, and the viscosity at 30°C is (coated - 4 cups) 14-15s, adds alkali solution to adjust the pH value to 6.1, adds 200 parts of triazine nitrogen-containing heterocyclic organic compounds and 1000 parts of urea, until the viscosity at 30°C is (coated - 4 cups) 15-16s;
[0041] S4: add alkali solution and adjust the pH value to 7.0, add 250 parts of the first auxiliary agent, add 1500 parts of urea, cool to 68°C, adjust the pH value to 7.5, add 1000 parts of urea, cool to 40°C, and obtain.
[0042] Example 2
[0043] The invention discloses a lignin-modified urea-formaldehyde resin for ENF-grade artificial board, wherein the raw materials for preparing the urea-formaldehyde resin are: formaldehyde (37 wt% aqueous solution), urea, triazine nitrogen-containing heterocyclic organic compound (melamine), alkali solution (sodium hydroxide aqueous solution, concentration of 32 wt%), acid solution (formic acid aqueous solution, concentration of 20 wt%), lignin, polyvinyl alcohol (Taiwan Changchun, BP-26), additives and water.
[0044] The auxiliary agent comprises a first auxiliary agent, a second auxiliary agent and a third auxiliary agent, wherein the first auxiliary agent is ammonium bicarbonate, the second auxiliary agent is sodium sulfate, and the third auxiliary agent comprises a 20 wt % sodium chloride aqueous solution.
[0045] A method for preparing lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels (raw materials are calculated by weight), comprising the following steps:
[0046] S1: Add 1000 parts of 37wt% formaldehyde, 50 parts of polyvinyl alcohol, 200 parts of lignin, and 1000 parts of water into a reactor, add alkali solution to adjust the pH value to 7.5, add 3000 parts of urea, 1000 parts of the first auxiliary agent, 5000 parts of the third auxiliary agent, 50 parts of the second auxiliary agent, and 250 parts of the triazine nitrogen-containing heterocyclic organic compound, and then heat to 92°C and keep warm for 30 minutes;
[0047] S2 is cooled to 88°C, and acid is added twice. The first time acid is added, the pH value is adjusted to 6.1, and the reaction is performed for 4 minutes. The second time acid is added, the pH value is adjusted to 5.1, and 100 parts of triazine nitrogen-containing heterocyclic organic compounds are added. The reaction is kept warm until the viscosity at 30°C is (coating-4 cups) 13-14s;
[0048] S3 adds alkali solution to adjust the pH value to 5.8, adds 1000 parts of urea, and the viscosity at 30°C is (coated - 4 cups) 14-15s, adds alkali solution to adjust the pH value to 6.1, adds 200 parts of triazine nitrogen-containing heterocyclic organic compounds and 1000 parts of urea, until the viscosity at 30°C is (coated - 4 cups) 15-16s;
[0049] S4: add alkali solution and adjust the pH value to 7.0, add 250 parts of the first auxiliary agent, add 1500 parts of urea, cool to 68°C, adjust the pH value to 7.5, add 1000 parts of urea, cool to 40°C, and obtain.
[0050] Example 3
[0051] The invention discloses a lignin-modified urea-formaldehyde resin for ENF-grade artificial board, wherein the raw materials for preparing the urea-formaldehyde resin are: formaldehyde (37 wt% aqueous solution), urea, triazine nitrogen-containing heterocyclic organic compound (melamine), alkali solution (sodium hydroxide aqueous solution, concentration of 32 wt%), acid solution (formic acid aqueous solution, concentration of 20 wt%), lignin, polyvinyl alcohol (Taiwan Changchun, BP-26), additives and water.
[0052] The auxiliary agent comprises a first auxiliary agent, a second auxiliary agent and a third auxiliary agent, wherein the first auxiliary agent is ammonium bicarbonate, the second auxiliary agent is sodium sulfate, and the third auxiliary agent comprises a 20 wt % sodium chloride aqueous solution.
[0053] A method for preparing lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels (raw materials are calculated by weight), comprising the following steps:
[0054] S1: Add 10,000 parts of 37 wt% formaldehyde, 50 parts of polyvinyl alcohol, 200 parts of lignin, and 1,000 parts of water into a reactor, add alkali solution to adjust the pH value to 7.5, add 3,500 parts of urea, 1,000 parts of the first auxiliary agent, 5,000 parts of the third auxiliary agent, 50 parts of the second auxiliary agent, and 250 parts of the triazine nitrogen-containing heterocyclic organic compound, and then heat to 92°C and keep warm for 30 minutes;
[0055] S2 is cooled to 88°C, and acid is added twice. The first time acid is added, the pH value is adjusted to 6.1, and the reaction is performed for 4 minutes. The second time acid is added, the pH value is adjusted to 5.1, and 100 parts of triazine nitrogen-containing heterocyclic organic compounds are added. The reaction is kept warm until the viscosity at 30°C is (coating-4 cups) 13-14s;
[0056] S3 adds alkali solution to adjust the pH value to 5.8, adds 1000 parts of urea, and the viscosity at 30°C is (coated - 4 cups) 14-15s, adds alkali solution to adjust the pH value to 6.1, adds 200 parts of triazine nitrogen-containing heterocyclic organic compounds and 1000 parts of urea, until the viscosity at 30°C is (coated - 4 cups) 15-16s;
[0057] S4: add alkali solution and adjust the pH value to 7.0, add 250 parts of the first auxiliary agent, add 1500 parts of urea, cool to 68°C, adjust the pH value to 7.5, add 1000 parts of urea, cool to 40°C, and obtain Example 4.
[0058] The invention discloses a lignin-modified urea-formaldehyde resin for ENF-grade artificial board, wherein the raw materials for preparing the urea-formaldehyde resin are: formaldehyde (37 wt% aqueous solution), urea, triazine nitrogen-containing heterocyclic organic compound (melamine), alkali solution (sodium hydroxide aqueous solution, concentration of 32 wt%), acid solution (formic acid aqueous solution, concentration of 20 wt%), lignin, polyvinyl alcohol (Taiwan Changchun, BP-26), additives and water.
[0059] The auxiliary agent comprises a first auxiliary agent, a second auxiliary agent and a third auxiliary agent, wherein the first auxiliary agent is ammonium bicarbonate, the second auxiliary agent is sodium sulfate, and the third auxiliary agent comprises a 20 wt % sodium chloride aqueous solution.
[0060] A method for preparing lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels (raw materials are calculated by weight), comprising the following steps:
[0061] S1: Add 1000 parts of 37wt% formaldehyde, 50 parts of polyvinyl alcohol, 500 parts of lignin, and 1000 parts of water into a reactor, add alkali solution to adjust the pH value to 7.5, add 3500 parts of urea, 1000 parts of the first auxiliary agent, 5000 parts of the third auxiliary agent, 50 parts of the second auxiliary agent, and 250 parts of the triazine nitrogen-containing heterocyclic organic compound, and then heat to 92°C and keep warm for 30 minutes;
[0062] S2 is cooled to 88°C, and acid is added twice. The first time acid is added, the pH value is adjusted to 6.1, and the reaction is performed for 4 minutes. The second time acid is added, the pH value is adjusted to 5.1, and 100 parts of triazine nitrogen-containing heterocyclic organic compounds are added. The reaction is kept warm until the viscosity at 30°C is (coating-4 cups) 13-14s;
[0063] S3 adds alkali solution to adjust the pH value to 5.8, adds 1000 parts of urea, and the viscosity at 30°C is (coated - 4 cups) 14-15s, adds alkali solution to adjust the pH value to 6.1, adds 200 parts of triazine nitrogen-containing heterocyclic organic compounds and 1000 parts of urea, until the viscosity at 30°C is (coated - 4 cups) 15-16s;
[0064] S4: add alkali solution and adjust the pH value to 7.0, add 250 parts of the first auxiliary agent, add 1500 parts of urea, cool to 68°C, adjust the pH value to 7.5, add 1000 parts of urea, cool to 40°C, and obtain.
[0065] Comparative Example 1
[0066] The specific implementation is the same as Example 1; the difference is that in step S1 of Comparative Example 1: the temperature is raised to 95° C. and kept warm for 35 minutes.
[0067] Comparative Example 2
[0068] The specific implementation method is the same as that of Example 1; the difference is that in step S1 of Comparative Example 2: the temperature is raised to 95° C., an acid solution is first added to adjust the pH of the system to 4.0, and then the temperature is kept for 25 minutes.
[0069] Performance testing methods and data
[0070] 1. According to GB / T 14732-2017 "Urea-formaldehyde, phenol-formaldehyde and melamine-formaldehyde resins for wood industry adhesives" and GB / T 14074-2017 "Test methods for adhesives and resins for wood industry", Examples 1 to 4 and Comparative Examples 1 to 2 were tested, and the quality indicators detected are shown in Table 1.
[0071] Table 1
[0072]
[0073] 2. According to the test method for bonding strength and formaldehyde emission in GB / T 17657-2013 "Test methods for physical and chemical properties of artificial boards and veneer artificial boards" - climate chamber method, examples 1 to 4 and comparative examples 1 to 2 were tested, using 40×40×2mm eucalyptus veneer, five layers, double-sided glue 380g / m 2 When adjusting the glue, add 35wt% flour, 200 mesh, and hot press for 13min at 125℃. The results are shown in Table 2.
[0074] Table 2
[0075] Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 <![CDATA[Formaldehyde emission (mg / m 3 )]]> 0.005 0.0010 0.005 0.008 0.010 0.012 Class III bonding strength (MPa) 1.00 1.15 0.95 0.88 1.18 1.20 Type II immersion stripping (≥5) 6 6 6 6 5 5
Claims
1. A lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels, It is characterized in that The components include: formaldehyde, urea, triazine nitrogen-containing heterocyclic organic compounds, alkali solution, acid solution, lignin polymer compounds, polyvinyl alcohol, additives and water.
2. The lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 1, It is characterized in that Calculated by weight, the components include: 8000-12000 parts of formaldehyde, 7500-10000 parts of urea, 1000-1500 parts of triazine nitrogen-containing heterocyclic organic compounds, 30-50 parts of alkali solution, 25-35 parts of acid solution, 200-500 parts of lignin polymer compounds, 50-100 parts of polyvinyl alcohol, 5000-13000 parts of additives, and 500-2000 parts of water.
3. The lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 2, It is characterized in that The triazine nitrogen-containing heterocyclic organic compound includes at least one of melamine, triallyl cyanurate, cyanuric chloride and trichloromelamine.
4. The lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 3, It is characterized in that The average polymerization degree of the polyvinyl alcohol is 1800-3000.
5. The lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 4, It is characterized in that The auxiliary agent includes a first auxiliary agent, a second auxiliary agent and a third auxiliary agent, the first auxiliary agent includes an ammonium salt, the second auxiliary agent includes at least one of a sodium salt and a magnesium salt, and the third auxiliary agent includes an aqueous solution of a sodium salt.
6. The lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 5, It is characterized in that The lignin-based polymer compound includes at least one of lignin, lignin sulfonate, and lignin carboxylate.
7. A method for preparing the lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 5 or 6, It is characterized in that The following steps are involved: S1, adding formaldehyde, polyvinyl alcohol, lignin polymer compound, and water, adding alkali solution to adjust the pH value to 7.2-8, adding 20-40wt% of urea, 20-40wt% of the first auxiliary agent, the third auxiliary agent, the second auxiliary agent, and 35-50wt% of the triazine nitrogen-containing heterocyclic organic compound to react; S2, cooling to 85-90°C, adding acid to adjust the pH value to 6.0-6.5, reacting for 2-10 minutes, then adding acid to adjust the pH value to 5.0-5.5, adding 15-25wt% of a total amount of a triazine nitrogen-containing heterocyclic organic compound, and carrying out a heat-insulating reaction; S3, adding alkali solution to adjust the pH value to 5.5-6.2, adding 10-20wt% of urea in total, adding alkali solution to adjust the pH value to 6.0-6.5, adding the remaining triazine nitrogen-containing heterocyclic organic compound and 10-20wt% of urea in total; S4, add alkali solution to adjust the pH value to 7.0-7.5, add the remaining first auxiliary agent, add a total of 15-30wt% urea, cool to 65-75°C, add alkali solution to adjust the pH value to 7.5-8.0, add the remaining urea, cool to 38-45°C, and obtain.
8. The method for preparing the lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 7, It is characterized in that The reaction temperature in step S1 is 88-94° C., and the reaction time is 25-35 min.
9. The method for preparing the lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to claim 8, It is characterized in that The product of the heat preservation reaction in step S2 has a viscosity of 12-15s at 30°C for 4 cups.
10. Use of the lignin-modified urea-formaldehyde resin for ENF-grade wood-based panels according to any one of claims 1 to 6, It is characterized in that Applicable to at least one of solid wood board, ecological board and blockboard.
Citation Information
Cited By
Modified urea-formaldehyde resin adhesive, preparation method and application of modified urea-formaldehyde resin adhesive in fiberboard
CN122381741A