Foam hole improving compound catalyst for rigid polyurethane foam and application method of foam hole improving compound catalyst

By using a composite catalyst of formic acid and N,N-dimethylcyclohexylamine in polyurethane hard foam materials, the problem of non-fine and unstable bubble cells is solved, and lower thermal conductivity and better pressure resistance are achieved Strength avoids concurrent bubbles and bursts, and improves material performance.

CN118930786APending Publication Date: 2024-11-12MEISIDE (JILIN) NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970793.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The bubble cells in existing polyurethane hard bubble materials are not delicate enough, which affects its thermal conductivity and compressive strength, and is prone to concurrent bubbles and bursts, resulting in unstable performance.

Method used

Using excess formic acid and N,N-dimethylcyclohexylamine in a mixing ratio of 15-25:30 as a compound catalyst, the gel catalyst is selected to maintain the foam-gel reaction equilibrium, and provides Heat vaporizes and stabilizes the cells.

Benefits of technology

It significantly improves the delicateness and stability of the bubble cells, reduces the thermal conductivity, improves the anti-aging performance, avoids the phenomenon of confluence and bubble breakage, and improves the overall performance of polyurethane hard foam materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930786A_ABST
    Figure CN118930786A_ABST
Patent Text Reader

Abstract

The invention relates to a foam hole improving compound catalyst for rigid polyurethane foam and an application method of the foam hole improving compound catalyst, and belongs to the technical field of preparation of polyurethane materials.Excessive formic acid solution is selected and mixed with N, N-dimethyl cyclohexylamine according to a certain mixing proportion, a gel catalyst can be selectively sealed through the acidity of the formic acid solution, and the foam hole improving compound catalyst can be used for improving the foam hole of rigid polyurethane foam. According to the foaming agent, the foaming agent is added into the formula, so that the whole foaming-gelation of the formula is kept balanced, heat vaporization can be better provided for a physical foaming agent in the formula due to the characteristic of reaction heat release, and in the later rapid gelation process, foam pores can be more stable, and the phenomena of foam merging, foam breaking and the like are avoided, so that the fineness of the foam pores is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane material preparation, and particularly relates to a composite catalyst for improving pores of polyurethane rigid foam and an application method thereof. Background Art

[0002] Catalysts are promoters of many chemical reactions, and this is also true in the field of polyurethane rigid foam applications. They can shorten reaction time, improve production efficiency, selectively promote positive reactions, and inhibit side reactions. In the production of polyurethane products, catalysts are a commonly used additive. Although the amount used is small, their effect is very large. In the chemical reaction of polyurethane foaming, there are two main reactions, foaming and gelling. Only when these two reactions reach a relative balance during the foaming process can relatively satisfactory products be made. With the development of industry, people have conducted more systematic and in-depth research on the variety, synthesis, catalytic mechanism, and formulation of polyurethane catalysts, and have developed a variety of catalysts that are suitable for different types and different uses, can adjust different reaction rates, and control the generation of different molecular structures.

[0003] Catalysts catalyze all reactions in the foaming process of the formula, but the overall catalytic activity and catalytic tendency will vary. Generally speaking, we will roughly divide the catalysts into three categories according to their catalytic tendency: foaming catalysts, gel catalysts, and balanced catalysts. In the foam preparation process, if the foaming reaction precedes the gel reaction, the viscosity increases too slowly, and most of the gas is completed before gelling, which will cause small bubbles to merge into large bubbles, thereby affecting the physical properties of the foam and even causing the foam to collapse; if gelling precedes foaming, its viscosity increases too fast, and it solidifies before a large number of bubbles are generated, resulting in poor fluidity and other properties. Normally, the overall activity of the foaming catalyst is higher than that of the gel catalyst. Therefore, in the foaming process, within the range of foaming-gel equilibrium, it is particularly important to adjust the catalyst to improve the pores to a certain extent without changing the reaction equilibrium.

[0004] Polyurethane foam is a three-dimensional network structure. The various properties of the foam are closely related to the fineness of the pores. Excellent pores can better wrap the foaming agent during foaming, thereby reducing the thermal conductivity and improving the thermal insulation performance; at the same time, the pores can directly affect the transverse / longitudinal compressive strength of the foam, reducing the differences in various directions; and its dimensional stability will also be improved.

[0005] Therefore, the prior art urgently needs a new technical solution to improve the pores and thereby improve the various properties of polyurethane foam. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a composite catalyst for improving the pores of polyurethane rigid foam and an application method thereof. An excess formic acid solution is selected and mixed with N,N-dimethylcyclohexylamine in a certain mixing ratio. The acidic selective closed gel catalyst can keep the overall foaming-gelling balance of the formula. The exothermic characteristic of the reaction can better provide heat vaporization for the physical foaming agent in the formula. In the later rapid gelation process, the pores can be made more stable, and the phenomena of combined bubbles and broken bubbles can be avoided, thereby maintaining the fineness of the pores.

[0007] A composite catalyst for improving pores of polyurethane rigid foam is prepared by mixing excess formic acid with N,N-dimethylcyclohexylamine in a certain mixing ratio of formic acid:N,N-dimethylcyclohexylamine=15-25:30 to obtain the catalyst.

[0008] The solvent used in the mixing process is a polar solvent, including water, ethylene glycol, diethylene glycol, and dipropylene glycol.

[0009] The invention discloses an application method of a composite catalyst for improving pores of polyurethane rigid foam. The composite catalyst for improving pores of polyurethane rigid foam is applied to prepare polyurethane rigid foam material. In the polyurethane rigid foam board or pipe formula, the premixed combined polyether and crude polymethylene polyphenyl polyisocyanate MDI are accurately weighed and premixed, and the catalyst is added in a gradient of 0g, 2.0g and 4.0g. The mixture is stirred for 8s at 2800r / min. After the foaming is completely gelled, the polyurethane rigid foam board with stable pores is obtained.

[0010] Through the above design scheme, the present invention can bring the following beneficial effects: a composite catalyst for improving the pores of polyurethane rigid foam and its application method, by adding a new catalyst to the original formula, the pores of polyurethane rigid foam material can be made finer. One of the most important characteristics of polyurethane foam is thermal conductivity, and the level of its thermal conductivity mostly depends on the thermal conductivity of the gas enclosed in the pores. The thermal conductivity of the foaming agent in polyurethane foaming is far superior to that of air. After vaporization, it is enclosed inside the pores. The fine and uniform pores can reduce its replacement with the outside air, thereby maintaining a low thermal conductivity of the finished foam product. At the same time, the excellent pore structure will make the pores more stable and its anti-aging performance will also be increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The present invention is further described below with reference to the accompanying drawings and specific embodiments:

[0012] Figure 1 The present invention is a schematic diagram of the preparation process of a composite catalyst for improving the pores of polyurethane rigid foam.

[0013] Figure 2This is a comparison chart of a specific implementation method of an application method of a composite catalyst for improving the pores of polyurethane rigid foam of the present invention under the condition of 930r / min for pipeline formulation.

[0014] Figure 3 This is a comparison chart of a specific implementation method of an application method of a composite catalyst for improving the pores of polyurethane rigid foam according to the present invention under the condition of 2800r / min for pipeline formulation.

[0015] Figure 4 This is a comparison chart of a specific implementation method of an application method of a composite catalyst for improving the pores of polyurethane rigid foam of the present invention under the condition of 930r / min for the plate formula.

[0016] Figure 5 This is a comparison chart of a specific implementation method of an application method of a composite catalyst for improving pores for polyurethane rigid foam of the present invention under the condition of 2800r / min for the plate formula. DETAILED DESCRIPTION

[0017] The present invention provides a composite catalyst for improving the pores of polyurethane rigid foam, such as Figure 1 As shown, select excessive formic acid solution, mix with N, N-dimethylcyclohexylamine according to a certain mixing ratio, can be by its acidic selective closed gel catalyst, make the overall foaming of the formula-gel keep balance, its reaction exothermic characteristics, can better provide heat vaporization for the physical foaming agent in the formula, and in the rapid gel process of the later stage, can make the pore more stable, avoid the occurrence and bubble, the phenomenon such as broken bubble, so as to maintain the fineness of the pore. In the composite of catalyst, it is necessary to select suitable solvent to ensure that the products therefrom are uniform liquid phase at room temperature, so that subsequent addition is used. Solvent used can be polar solvents such as water, ethylene glycol, diethylene glycol, dipropylene glycol, and preferably diethylene glycol in the present invention.

[0018] The composite catalyst system used in the present invention is suitable for a polyurethane rigid foam system.

[0019] The test formula used in the present invention is a conventional low-index plate formula and pipe formula.

[0020] The present invention uses flat foaming, and the curing time is 10 minutes.

[0021] The test environment in the present invention should meet the requirements of GB / T2918-1998, with a temperature of 22°C ± 1°C and a relative humidity of 50% ± 5%.

[0022] The experimental steps in the present invention are as follows:

[0023] Choose a 50ml transparent glass bottle with a PET sealing cap to ensure good sealing during the catalyst compounding and mixing process and facilitate stability observation;

[0024] In the pipeline formula, the pre-mixed combined polyether and crude MDI are accurately weighed, and the compound catalyst is added in a gradient of 2.0g and 4.0g. The three are then mixed synchronously with a stirrer at a stirring speed of 2800r / min and a stirring time of 8s. The reaction time is tested in a fume hood;

[0025] After the foam is fully expanded, cut it in the middle and observe the fineness of the pores.

[0026] Adjust the stirrer to different speeds and repeat the above test to test the reproducibility of the improvement of foam cells by this catalyst at different speeds;

[0027] Under different test conditions, the differences in pore size were compared with those of the blank control group;

[0028] Repeat the above steps in the sheet formulation to test the improvement of the pores in different formulations.

[0029] Specifically, Figure 2-Figure 5 As shown, the experimental methods in the following control samples and examples without special description are all conventional operations, and the reagents used are commonly available on the market.

[0030] Comparative Example 1: Preparation of composite catalyst

[0031] 30 g of N, N-dimethylcyclohexylamine was added dropwise to 30 g of diethylene glycol. After mixing evenly, 20 g of formic acid was added dropwise to the mixture in a gradient manner. The temperature of the mixture was controlled not to exceed 50°C. The mixture was stirred and mixed continuously until it became a uniform and stable liquid.

[0032] Comparative Example 2: Test results of bubble holes in pipe formulas at different rotation speeds

[0033] Table 1 shows the typical polyurethane formulation for pipes:

[0034] Raw material name Model or specification Proportion Polyether polyols Sucrose initiator, five functional groups, hydroxyl value 430~470mgKOH / g 60pbw Polyether polyols Sorbitol initiator, hexafunctional, hydroxyl value 480~510mgKOH / g 25pbw Polyether polyols Glycerol initiator, trifunctional, hydroxyl value 450~500mgKOH / g 10pbw Silicone surfactant Maysta8860 2~3pbw water Deionized water 2pbw catalyst Amine catalysts 1.5~2pbw Compound Catalyst Vary Vary Foaming agent (141B) ≥99.9% 20~25pbw Crude MDI NCOcontent%:30.5-32mPa.s:170-250(25℃) 120~125pbw

[0035] 60 g of the combined polyether in the above formula (i.e., all raw materials except MDI are stirred and mixed in proportion) is taken into a 500 ml foaming cup, 66 g of crude MDI is added, and the mixture is stirred and mixed for 8 s at different speeds of 930 r / min and 2800 r / min, and its reactivity time is tested, as shown in Table 2.

[0036] Table 2

[0037] Speed Number of catalysts added Milky time(s) Gel time (s) Non-stick time(s) 930r / min 0 16 113 165 2800r / min 0 15 110 160

[0038] Comparative Example 3: Test results of foam cells in sheet materials at different rotation speeds

[0039] Table 3 shows the typical polyurethane formula for panels:

[0040] Raw material name Model or specification Proportion Polyether polyols Sucrose initiator, five functional groups, hydroxyl value 430~470mgKOH / g 35pbw Polyether polyols Glycerol initiator, trifunctional, hydroxyl value 450~500mgKOH / g 20pbw Polyester polyols Benzene ring polyester, difunctional group, hydroxyl value 230~270mgKOH / g 40pbw Silicone surfactant Maysta8860 2~3pbw water Deionized water 1.5~2pbw catalyst Amine catalysts 2~3pbw Compound Catalyst Vary Vary Foaming agent (141B) ≥99.9% 20~25pbw Crude MDI NCOcontent%:30.5-32mPa.s:170-250(25℃) 145~150pbw

[0041] 60 g of the combined polyether in the above formula (i.e., all raw materials except MDI are stirred and mixed in proportion) is taken into a 500 ml foaming cup, and 72 g of crude MDI is added. After stirring and mixing at different speeds of 930 r / min and 2800 r / min for 8 s, the reactivity time is tested, as shown in Table 4.

[0042] Table 4

[0043] Speed Number of catalysts added Milky time(s) Gel time (s) Non-stick time(s) 930r / min 0 14 71 113 2800r / min 0 12 69 110

[0044] Example 1: The test results of the bubble holes of the pipe formula under different rotation speeds are shown in Table 5:

[0045] Table 5

[0046]

[0047] Combination Figure 2 and Figure 3 , and thermal conductivity, under different rotation speeds, the composite catalyst has the same improvement effect on the cell fineness and thermal conductivity of the overall foam, and the thermal conductivity has decreased. It has a promoting effect on the thermal insulation performance of the later pipeline foam products.

[0048] Example 2: The foam cell test results of the plate formula under different rotation speeds are shown in Table 6:

[0049] Table 6

[0050]

[0051] Combination Figure 4 and Figure 5 , and thermal conductivity, under different rotation speeds, the composite catalyst has the same improvement effect on the cell fineness and thermal conductivity of the overall foam, and the thermal conductivity has decreased. It has a promoting effect on the thermal insulation and heat insulation function of the later foam products.

Claims

1. A composite catalyst for improving the pores of polyurethane rigid foam, characterized by: Formic acid is mixed with N,N-dimethylcyclohexylamine in a ratio of formic acid:N,N-dimethylcyclohexylamine=15-25:30 to obtain a catalyst.

2. The composite catalyst for improving cells of a polyurethane rigid foam according to claim 1, characterized in that: The solvent used in the mixing process is a polar solvent, including water, ethylene glycol, diethylene glycol, and dipropylene glycol.

3. An application method of a composite catalyst for improving the pores of polyurethane rigid foam, characterized in that: A polyurethane rigid foam material is prepared using a composite catalyst for improving the pores of a polyurethane rigid foam as described in claim 1. In the polyurethane rigid foam board or pipe formula, the premixed combined polyether and crude MDI polymethylene polyphenyl polyisocyanate are accurately weighed, and the catalyst is added in a gradient of 0g, 2g, and 4g. The mixture is stirred at 2800r / min for 8s, and after the foaming is completely gelled, a polyurethane rigid foam board with stable pores is obtained.