High-hydrophilicity polyurethane filter cotton and preparation method thereof

By modifying cellulose to prepare a network structure and introducing polyurethane materials, the problems of insufficient hydrophilicity and temperature resistance of polyurethane filter cotton were solved, achieving performance improvement and application expansion.

CN118930795APending Publication Date: 2024-11-12JIANGSU YUHUIHONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411265136.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Polyurethane filter cotton has poor hydrophilicity and insufficient temperature resistance, which limits its application range.

Method used

By modifying cellulose and introducing 1,3-bis(chloromethyl)tetramethyldisiloxane and tetraethylene glycol mono-p-toluenesulfonate, a network structure cellulose was prepared and introduced into polyurethane materials. Combined with polyether polyol, catalyst and diisocyanate, it was foamed to form a highly hydrophilic polyurethane filter cotton.

Benefits of technology

This improved the hydrophilicity, high-temperature resistance, and mechanical properties of polyurethane filter cotton, expanding its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses high-hydrophilicity polyurethane filter cotton and a preparation method thereof, and belongs to the technical field of polyurethane, the high-hydrophilicity polyurethane filter cotton comprises the following raw materials by weight: 20-30 parts of polyether polyol, 5-8 parts of modified cellulose, 5-15 parts of diisocyanate, 0.1-0.3 part of a catalyst, 0.5-1 part of an organosilicon foam stabilizer and 1-3 parts of water; according to the prepared high-hydrophilicity polyurethane filter cotton, on the basis that the excellent performance of original polyurethane filter cotton is kept, the hydrophilicity, the high-temperature resistance and the mechanical performance of the filter cotton are improved, the application range of the filter cotton is widened, and the high-hydrophilicity polyurethane filter cotton has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane, and in particular relates to a highly hydrophilic polyurethane filter cotton and a preparation method thereof. Background Art

[0002] Polyurethane is a polymer material with excellent compression resistance, tear resistance, water resistance and chemical stability. Polyurethane filter cotton is a filter cotton with a microporous structure made of polyurethane material. It has the characteristics of high filtration efficiency, good water resistance, good chemical resistance and long service life. Therefore, it is often used in air purification, water treatment, food processing and pharmaceutical manufacturing.

[0003] However, since polyurethane itself is hydrophobic and has poor high temperature resistance, the polyurethane filter cotton produced has poor hydrophilicity and is not easily wetted by water. Poor hydrophilicity will reduce its efficiency in filtering water-based pollutants, and is not conducive to its use in situations where water absorption is required, and affects its compounding and bonding with other materials; poor temperature resistance will cause the filter cotton to shrink and deform in high temperature environments, thereby limiting the application range of polyurethane filter cotton. Therefore, how to modify polyurethane filter cotton, improve the performance of polyurethane filter cotton, and expand its application field is an urgent problem to be solved. Summary of the invention

[0004] To solve the above problems, the purpose of the present invention is to provide a highly hydrophilic polyurethane filter cotton and a preparation method thereof.

[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions: A highly hydrophilic polyurethane filter cotton is composed of the following raw materials, measured in parts by weight: 20-30 parts of polyether polyol, 5-8 parts of modified cellulose, 5-15 parts of diisocyanate, 0.1-0.3 parts of catalyst, 0.5-1 parts of organosilicon foam stabilizer and 1-3 parts of water; The modified cellulose is prepared by modifying cellulose with 1,3-bis(chloromethyl)tetramethyldisiloxane and triethylene glycol mono-p-toluenesulfonate.

[0006] The catalyst is triethylenediamine, dimethylethanolamine, dibutyltin dilaurate or stannous octoate.

[0007] The diisocyanate is toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate.

[0008] The modified cellulose is prepared according to the following method: Add cellulose to a mixed solvent of lithium chloride-dimethylacetamide, stir and dissolve, then add 1,3-bis(chloromethyl)tetramethyldisiloxane and sodium hydride, react at 25-50°C for 3-5 hours, add tetraethylene glycol mono-p-toluenesulfonate and continue the reaction for 12-20 hours. After the reaction is completed, add water to the reaction solution to quench the reaction, then distill under reduced pressure to remove the solvent, filter the obtained residue, wash the obtained filter cake with acetone for 3-5 times, and dry to obtain modified cellulose.

[0009] The mass ratio of the cellulose, lithium chloride-dimethylacetamide, 1,3-bis(chloromethyl)tetramethyldisiloxane, sodium hydride, tetraethylene glycol mono-p-toluenesulfonate and water is 1:10-20:1.2-2:0.8-1.5:3-6:5-8.

[0010] The mass concentration of lithium chloride in the lithium chloride-dimethylacetamide mixed solvent is 5-10%.

[0011] The method for preparing the highly hydrophilic polyurethane filter cotton comprises the following steps: In parts by weight, 20-30 parts of polyether polyol, 5-8 parts of modified cellulose, 0.1-0.3 parts of catalyst, 0.5-1 parts of silicone foam stabilizer and 1-3 parts of water are added into a stirrer, mixed at 25°C and 2000-4000 r / min for 5-10 seconds, 5-15 parts of diisocyanate are added and mixed for 5-10 seconds, the obtained mixture is added into a mold and foamed for 20-24 hours to obtain a highly hydrophilic polyurethane filter cotton.

[0012] Compared with the prior art, the present invention has the following advantages: The highly hydrophilic polyurethane filter cotton of the present invention utilizes 1,3-bis(chloromethyl)tetramethyldisiloxane and tetraethylene glycol mono-p-toluenesulfonate to modify cellulose to prepare a cellulose mesh structure, and then the modified cellulose is introduced into a polyurethane material, the main chain of the polyurethane is wrapped in the cellulose mesh structure, the cellulose mesh structure can be more hydrophilic and water-retaining, thereby improving the water absorption rate of the filter cotton; the introduction of the side chain ether chain can further improve the hydrophilicity and mechanical properties of the polyurethane filter cotton; the introduction of siloxane can improve the high temperature resistance and biocompatibility of the material, thereby improving the composite and bonding performance with other materials.

[0013] The highly hydrophilic polyurethane filter cotton prepared by the invention improves the hydrophilicity, high temperature resistance and mechanical properties of the polyurethane filter cotton while maintaining the excellent performance of the original filter cotton, thereby expanding its application range and having good application prospects. DETAILED DESCRIPTION

[0014] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.

[0015] Example 1 Preparation of modified cellulose: 0.1 kg of cellulose was added to 1 kg of a mixed solvent of lithium chloride-dimethylacetamide with a mass concentration of 5%, and after stirring to dissolve, 0.12 kg of 1,3-bis(chloromethyl)tetramethyldisiloxane and 0.08 kg of sodium hydride were added thereto. After reacting at 25°C for 5 hours, 0.3 kg of tetraethylene glycol mono-p-toluenesulfonate was added and the reaction was continued for 12 hours. After the reaction was completed, 0.5 kg of water was added to the reaction solution to quench the reaction, and the solvent was removed by distillation under reduced pressure. The obtained residue was filtered, and the obtained filter cake was washed 3 times with acetone and dried to obtain modified cellulose.

[0016] 2 kg of polyether polyol, 0.5 kg of modified cellulose, 0.01 kg of triethylenediamine, 0.05 kg of silicone foam stabilizer and 0.1 kg of water were added into a stirrer and mixed at 25°C and 2000 r / min for 10 seconds. Then 0.5 kg of toluene diisocyanate was added and mixed for 5 seconds. The resulting mixture was added into a mold and foamed for 20 hours to obtain a highly hydrophilic polyurethane filter cotton.

[0017] Example 2 Preparation of modified cellulose: 0.1 kg of cellulose was added to 1.2 kg of a mixed solvent of lithium chloride-dimethylacetamide with a mass concentration of 6%, and after stirring to dissolve, 0.13 kg of 1,3-bis(chloromethyl)tetramethyldisiloxane and 0.1 kg of sodium hydride were added thereto. After reacting at 35°C for 4.5 hours, 0.4 kg of tetraethylene glycol mono-p-toluenesulfonate was added and the reaction was continued for 14 hours. After the reaction was completed, 0.6 kg of water was added to the reaction solution to quench the reaction, and the solvent was removed by distillation under reduced pressure. The obtained residue was filtered, and the obtained filter cake was washed 5 times with acetone and dried to obtain modified cellulose.

[0018] 2.2 kg of polyether polyol, 0.6 kg of modified cellulose, 0.015 kg of dibutyltin dilaurate, 0.06 kg of silicone foam stabilizer and 0.15 kg of water were added into a stirrer and mixed at 25°C and 2500 r / min for 8 seconds. Then 0.7 kg of isophorone diisocyanate was added and mixed for 6 seconds. The resulting mixture was added into a mold and foamed for 21 hours to obtain a highly hydrophilic polyurethane filter cotton.

[0019] Example 3 Preparation of modified cellulose: 0.1 kg of cellulose was added to 1.5 kg of a mixed solvent of lithium chloride-dimethylacetamide with a mass concentration of 7%, and after stirring to dissolve, 0.15 kg of 1,3-bis(chloromethyl)tetramethyldisiloxane and 0.12 kg of sodium hydride were added thereto. After reacting at 40°C for 4 hours, 0.5 kg of tetraethylene glycol mono-p-toluenesulfonate was added and the reaction was continued for 16 hours. After the reaction was completed, 0.7 kg of water was added to the reaction solution to quench the reaction, and the solvent was removed by distillation under reduced pressure. The obtained residue was filtered, and the obtained filter cake was washed 5 times with acetone and dried to obtain modified cellulose.

[0020] 2.5 kg of polyether polyol, 0.7 kg of modified cellulose, 0.02 kg of stannous octoate, 0.08 kg of silicone foam stabilizer and 0.2 kg of water were added into a stirrer and mixed at 25°C and 3000 r / min for 8 seconds. Then 1 kg of diphenylmethane diisocyanate was added and mixed for 8 seconds. The resulting mixture was added into a mold and foamed for 22 hours to obtain a highly hydrophilic polyurethane filter cotton.

[0021] Example 4 Preparation of modified cellulose: 0.1 kg of cellulose was added to 1.8 kg of a mixed solvent of lithium chloride-dimethylacetamide with a mass concentration of 8%, and after stirring to dissolve, 0.18 kg of 1,3-bis(chloromethyl)tetramethyldisiloxane and 0.14 kg of sodium hydride were added thereto. After reacting at 45°C for 3.5 hours, 0.55 kg of tetraethylene glycol mono-p-toluenesulfonate was added and the reaction was continued for 18 hours. After the reaction was completed, 0.75 kg of water was added to the reaction solution to quench the reaction, and the solvent was removed by distillation under reduced pressure. The obtained residue was filtered, and the obtained filter cake was washed 5 times with acetone and dried to obtain modified cellulose.

[0022] 2.8 kg of polyether polyol, 0.75 kg of modified cellulose, 0.025 kg of dimethylethanolamine, 0.08 kg of silicone foam stabilizer and 0.25 kg of water were added into a stirrer and mixed at 25°C and 3500 r / min for 6 seconds. Then 1.3 kg of diphenylmethane diisocyanate was added and mixed for 9 seconds. The resulting mixture was added into a mold and foamed for 23 hours to obtain a highly hydrophilic polyurethane filter cotton.

[0023] Example 5 Preparation of modified cellulose: 0.1 kg of cellulose was added to 2 kg of a 10% mass concentration of lithium chloride-dimethylacetamide mixed solvent, stirred to dissolve, and then 0.2 kg of 1,3-bis(chloromethyl)tetramethyldisiloxane and 0.15 kg of sodium hydride were added thereto. After reacting at 50°C for 3 hours, 0.6 kg of tetraethylene glycol mono-p-toluenesulfonate was added and the reaction was continued for 20 hours. After the reaction was completed, 0.8 kg of water was added to the reaction solution to quench the reaction, and the solvent was removed by distillation under reduced pressure. The obtained residue was filtered, and the obtained filter cake was washed 4 times with acetone and dried to obtain modified cellulose.

[0024] 3 kg of polyether polyol, 0.8 kg of modified cellulose, 0.03 kg of triethylenediamine, 0.1 kg of silicone foam stabilizer and 0.3 kg of water were added into a stirrer and mixed at 25°C and 4000 r / min for 5 seconds. Then 1.5 kg of isophorone diisocyanate was added and mixed for 10 seconds. The resulting mixture was added into a mold and foamed for 24 hours to obtain a highly hydrophilic polyurethane filter cotton.

[0025] Example 6 Preparation of modified cellulose: 0.1 kg of cellulose was added to 2 kg of a 5% by mass concentration of lithium chloride-dimethylacetamide mixed solvent, stirred to dissolve, and then 0.15 kg of 1,3-bis(chloromethyl)tetramethyldisiloxane and 0.15 kg of sodium hydride were added thereto. After reacting at 50°C for 5 hours, 0.6 kg of tetraethylene glycol mono-p-toluenesulfonate was added and the reaction was continued for 12 hours. After the reaction was completed, 0.8 kg of water was added to the reaction solution to quench the reaction, and the solvent was removed by distillation under reduced pressure. The obtained residue was filtered, and the obtained filter cake was washed 5 times with acetone and dried to obtain modified cellulose.

[0026] 3 kg of polyether polyol, 0.5 kg of modified cellulose, 0.03 kg of dibutyltin dilaurate, 0.07 kg of silicone foam stabilizer and 0.3 kg of water were added into a stirrer and mixed at 25°C and 3000 r / min for 10 seconds. Then 1 kg of isophorone diisocyanate was added and mixed for 10 seconds. The resulting mixture was added into a mold and foamed for 23 hours to obtain a highly hydrophilic polyurethane filter cotton.

[0027] Comparative Example 1: 2.5 kg of polyether polyol, 0.02 kg of stannous octoate, 0.08 kg of silicone foam stabilizer and 0.2 kg of water were added into a stirrer and mixed at 25°C and 3000 r / min for 8 s. Then 1 kg of diphenylmethane diisocyanate was added and mixed for 8 s. The obtained mixture was added into a mold and foamed for 22 hours to obtain a polyurethane filter cotton.

[0028] The highly hydrophilic polyurethane filter cotton prepared in Examples 1 to 6 and the polyurethane filter cotton prepared in Comparative Example 1 were subjected to performance tests, wherein the apparent density was tested according to the method in GB / T6343-2009; the open porosity was tested according to the method in GB / T10799-2008; the water absorption rate test: the polyurethane sponge was cut into samples with a specification of 100 mm×100 mm×100 mm, and the mass was recorded as m 1 , submerge the sample in water for 30 minutes, take it out, absorb the surface water with filter paper, and record the mass as m 2 , water absorption rate = (m 2 -m 1 ) / m 1 ×100%; the tensile strength and elongation are tested according to the method in GB / T6344-2008, and the test results are shown in Table 1.

[0029] Table 1 Polyurethane filter cotton performance results

[0030] It can be seen from the results in Table 1 that the highly hydrophilic polyurethane filter cotton prepared in the present invention has higher hydrophilicity, temperature resistance and excellent mechanical properties than the comparative example, and can be suitable for different application fields.

[0031] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. A highly hydrophilic polyurethane filter cotton, Features: The composition is composed of the following raw materials in parts by weight: 20-30 parts of polyether polyol, 5-8 parts of modified cellulose, 5-15 parts of diisocyanate, 0.1-0.3 parts of catalyst, 0.5-1 parts of organosilicon foam stabilizer and 1-3 parts of water; The modified cellulose is prepared by modifying cellulose with 1,3-bis(chloromethyl)tetramethyldisiloxane and triethylene glycol mono-p-toluenesulfonate.

2. The highly hydrophilic polyurethane filter cotton according to claim 1, Features: The catalyst is triethylenediamine, dimethylethanolamine, dibutyltin dilaurate or stannous octoate.

3. The highly hydrophilic polyurethane filter cotton according to claim 1, Features: The diisocyanate is toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate.

4. The highly hydrophilic polyurethane filter cotton according to claim 1, Features: The modified cellulose is prepared according to the following method: Add cellulose to a mixed solvent of lithium chloride-dimethylacetamide, stir and dissolve, then add 1,3-bis(chloromethyl)tetramethyldisiloxane and sodium hydride, react at 25-50°C for 3-5 hours, add tetraethylene glycol mono-p-toluenesulfonate and continue the reaction for 12-20 hours. After the reaction is completed, add water to the reaction solution to quench the reaction, then distill under reduced pressure to remove the solvent, filter the obtained residue, wash the obtained filter cake with acetone for 3-5 times, and dry to obtain modified cellulose.

5. The highly hydrophilic polyurethane filter cotton as claimed in claim 4, Features: The mass ratio of the cellulose, lithium chloride-dimethylacetamide, 1,3-bis(chloromethyl)tetramethyldisiloxane, sodium hydride, tetraethylene glycol mono-p-toluenesulfonate and water is 1:10-20:1.2-2:0.8-1.5:3-6:5-8.

6. The highly hydrophilic polyurethane filter cotton as claimed in claim 4, Features: The mass concentration of lithium chloride in the lithium chloride-dimethylacetamide mixed solvent is 5-10%.

7. A method for preparing the highly hydrophilic polyurethane filter cotton according to claim 1, Features: The following steps are involved: In parts by weight, 20-30 parts of polyether polyol, 5-8 parts of modified cellulose, 0.1-0.3 parts of catalyst, 0.5-1 parts of silicone foam stabilizer and 1-3 parts of water are added into a stirrer, mixed at 25°C and 2000-4000 r / min for 5-10 seconds, 5-15 parts of diisocyanate are added and mixed for 5-10 seconds, the obtained mixture is added into a mold and foamed for 20-24 hours to obtain a highly hydrophilic polyurethane filter cotton.

Citation Information

Cited By

  • Sponge water treatment system

    CN120204780A