Low-density and high-comfort polyurethane foam plastic as well as preparation method and application thereof

By using specific ratio polyether polyols and isocyanate components to prepare low-density polyurethane foam, the hysteresis loss and comfort problems caused by density reduction are solved, and the low-density, high comfort and low-hysteresis loss polyurethane foam is achieved. Suitable for car seat applications.

CN118930801APending Publication Date: 2024-11-12CHANGHUA CHEMICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411140057.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the product hysteresis loss and the comfort of the product caused by the reduction of product density are high, especially in automotive seat applications, it is difficult to maintain low hysteresis loss and high comfort while meeting low density.

Method used

Use low-density, high-comfort polyurethane foam composed of components A and component B. Component A includes a specific range of polyether polyols, Mannich polyether polyols, crosslinkers, and amine-type reaction types. Catalyst, foam stabilizer and foaming agent, component B is a polyfunctional isocyanate, prepared by casting with high pressure or low pressure foaming machine to obtain a polyurethane foam with low density and low hysteresis loss.

Benefits of technology

It achieves low density (35.2~44.8kg/m3), low hysteresis loss (15.2~16.7%) and reduced vibration transmittance at around 5Hz, improving product comfort and meeting the performance requirements of car seats.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930801A_ABST
    Figure CN118930801A_ABST
Patent Text Reader

Abstract

The invention relates to low-density and high-comfort polyurethane foam plastic as well as a preparation method and application thereof, and mainly solves the problems that in the prior art, after the density of the polyurethane foam plastic is reduced, the hysteresis loss rate of a product becomes high, the resonant frequency moves to high frequency, and the comfort of the product becomes poor. The low-density and high-comfort polyurethane foam plastic is composed of a component A and a component B, the weight ratio of the component A to the component B is 100: (40-70), the component A is prepared from the following components in parts by weight: 40-100 parts of polyether polyol A1, 0-30 parts of Mannich polyether polyol A2, 0-30 parts of polymer polyol A3, 0.1-1.0 part of a cross-linking agent and 0.1-1.0 part of an amine reaction type catalyst, and the component B is prepared from the following components in parts by weight: 0.1-1.0 part of a cross-linking agent and 0.1-1.0 part of an amine reaction type catalyst. The foam stabilizer accounts for 0.5-2.0 parts, the water accounts for 3.0-4.5 parts, and the foaming agent accounts for 1-20 parts; the component B is a mixture of toluene diisocynate and diphenylmethane diisocyanate, so that the problem is well solved, and the automobile seat can be applied to the automobile seat industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-density, high-comfort polyurethane foam plastic and a preparation method and application thereof. Background Art

[0002] Automotive polyurethane is mainly used in automotive dashboards, seat cushions, backrests, headrests, doors, armrests, steering wheel assemblies, automotive roofs, door inner panels and seals. It is the most promising and important material for the plasticization of automobiles. At present, the development direction of the world's automobiles (mainly sedans and new energy vehicles) is lightweight (that is, the product density is required to be low). Lightweighting is to improve fuel combustion efficiency and reduce automobile exhaust emissions, and it is also an important technical measure to achieve automobile energy conservation and emission reduction. The plasticization and polyurethaneization of automotive materials, replacing steel with plastic, is an inevitable trend and important technical approach for the development of lightweight automobiles.

[0003] High-resilience polyurethane foam is a kind of polyurethane foam material. It has various properties such as mechanical properties, thermal insulation and vibration absorption properties according to the application requirements. In particular, it is required to have high resilience, ride comfort and other comfort in vehicle seat cushions. In order to improve the vibration absorption characteristics near 6Hz (about 4-8Hz), which is usually regarded as the resonance point of the human body, the structure of the main components of polyurethane foam raw materials is re-examined, and attempts are made to reduce the resonance frequency and resonance magnification of polyurethane foam. In order to reduce the resonance frequency and resonance magnification, increasing density and weight are effective. However, as people's understanding of "lightweight" becomes more and more in-depth, in the direction of automobile seats, in order to meet the goal of lightweight seats, two methods are usually adopted. One is to reduce the core density of the foam as much as possible while ensuring that the foam performance does not decrease; the other is to reduce the thickness of the foam as much as possible while ensuring that the foam performance does not decrease. However, as the seat density decreases, the performance of the product also decreases. After the seat thickness is reduced, the resonance frequency will move to high frequency, and the transmittance above 5Hz will increase significantly, causing discomfort to passengers. The comfort of the product is characterized by hysteresis loss, rebound rate and vibration transmittance.

[0004] The Chinese patent application number 2019109419174 discloses a low-density, high-performance, high-resilience foam plastic and its preparation method and application. By adopting a low-density, high-performance, high-resilience polyurethane foam plastic, composed of component A and component B, the weight ratio of component A to component B is 100:50-80, wherein: component A, in parts by weight, includes 60-100 parts of polyether polyol, 1-5 parts of cross-linking agent, 1-5.5 parts of non-volatile reaction catalyst, 0.3-1.5 parts of silicone foam stabilizer, and 2.5-6 parts of water; component B is a technical solution of a carbamate-modified MDI prepolymer with an isocyanate content of 22-33%, and the obtained product density is 38-42.6kg / m 3However, the patent does not describe the resonant frequency and hysteresis loss performance that characterize comfort.

[0005] Chinese patent CN110835400A discloses a high-resilience polyurethane foam with high comfort, low hysteresis loss and low VOC, and its preparation method and application. By adopting a high-resilience polyurethane foam with high comfort, low hysteresis loss and low VOC, composed of component A and component B, the weight ratio of component A to component B is 100:30-55, wherein component A includes the following components in parts by weight: 150-70 parts of polyether polyol A, 230-50 parts of polymer polyol A, 0.5-3 parts of cross-linking agent, 0.5-2.5 parts of non-volatile reaction catalyst, 0.3-1.5 parts of low-fogging silicone foam stabilizer, 1.5-2.5 parts of water, and 0.5-5 parts of cell opener; component B is a mixture of toluene diisocyanate and diphenylmethane diisocyanate, and the obtained product density is 47-54 kg / m 3 However, the patent does not describe the resonant frequency that characterizes comfort.

[0006] The general performance requirements of polyurethane foam plastics are shown in Table 1 below:

[0007] Table 1 Test items and index requirements for polyurethane foam plastics

[0008] Test items Test Standards Index requirements density ISO845-2006 The lower the density, the lower the cost Hysteresis loss ISO2439-2009 The lower the hysteresis loss, the higher the comfort Rebound rate ISO8307-2008 General requirement>50% Tensile Strength ISO1798-2008 Generally required ≥100kPa Elongation at break ISO1798-2008 Generally required ≥100% Compression hardness ISO3386-2010 Generally set at 5~9kPa Compression set ISO1856-2007 Generally required ≤8% odor VDA270 Generally required ≤3.0 Summary of the invention

[0009] One of the technical problems to be solved by the present invention is the problem in the prior art that the hysteresis loss of the product becomes higher and the comfort becomes worse due to the reduction of the product density. A low-density, high-comfort polyurethane foam plastic is provided. The product has the advantages of low hysteresis and good comfort while meeting the requirements of a lower density.

[0010] The second technical problem to be solved by the present invention is to provide a method for preparing a low-density, high-comfort urethane foam plastic corresponding to the first technical problem to be solved.

[0011] The third technical problem to be solved by the present invention is to provide an application of low-density, high-comfort polyurethane foam plastic corresponding to the first technical problem to be solved.

[0012] In order to solve one of the above technical problems, the technical solution adopted by the present invention is as follows: a low-density, high-comfort polyurethane foam plastic, comprising: composed of component A and component B, component A and component B are calculated in a weight percentage of 100:40-70, wherein component A, calculated in parts by weight, comprises the following components: 40-100 parts of polyether polyol A1, 0-30 parts of Mannich polyether polyol A2, 0-30 parts of polymer polyol A3, 0.1-1.0 parts of cross-linking agent, 0.1-1.0 parts of amine reaction catalyst, 0.5-2.0 parts of foam stabilizer, 3.0-4.5 parts of water, and 1-20 parts of foaming agent; component B is various multifunctional aliphatic, alicyclic and aromatic isocyanates. The polyether polyol A1 is prepared by polymerization of active hydrogen compounds and olefin oxides using organic phosphorus alcohol salts as catalysts, and has a molecular weight of 4000-15000, a functionality of 2-6, a molecular weight distribution coefficient of 1.0-1.06, an unsaturation of ≤0.04 mmol / g, and a primary hydroxyl content of more than 85%. The Mannich polyether polyol A2 is gradually synthesized by Mannich reaction, has an aromatic ring structure, a hydroxyl value of 240-390 mgKOH / g, and a functionality of 2-4. The polymer polyol A3 has a hydroxyl value of 15-28 mgKOH / g, a functionality of 2-4, and a solid content of 27-47%.

[0013] In the above technical scheme, the active hydrogen compound of the polyether polyol A1 in the component A is an organic compound containing hydroxyl groups, selected from hydroxy alcohols, sugars or their derivatives having 2 to 20 carbon atoms and 1 to 8 hydroxyl groups, or polyether polyols having 2 to 8 hydroxyl groups and a number average molecular weight of 200 to 5000; the oxidized olefin is selected from at least one of ethylene oxide, propylene oxide, 1,2-butylene oxide or styrene oxide.

[0014] In the above technical solution, the molecular weight of the polyether polyol A1 in component A is 6000-10000 and the functionality is 2-4.

[0015] In the above technical scheme, the cross-linking agent in component A is selected from one or a combination of diethanolamine and triethanolamine; the amine reaction catalyst is selected from one or a combination of ZF-10, Z-130, DMEA, and NE-1070; the foam stabilizer is selected from one or a combination of low-atomization B-8734, B-8738, and B-8715.

[0016] In the above technical solution, the foaming agent in component A is selected from one or a combination of 245FA and LBA. Due to the particularity of these two components, the foaming agent has little harm to the human body and is very friendly to the environment.

[0017] In the above technical solution, the component B is selected from one or a combination of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), xylene diisocyanate, and polymethylene polyphenylene polyisocyanate.

[0018] To solve the second technical problem, the technical solution adopted by the present invention is as follows: a preparation scheme of low-density, high-comfort polyurethane foam plastics, comprising the following steps:

[0019] (1) Preparation of component A: In a container, according to weight parts, 140-100 parts of polyether polyol A, 20-30 parts of Mannich polyether polyol A, 30-30 parts of polymer polyol A, 0.1-1.0 parts of crosslinking agent, 0.1-1.0 parts of amine reaction catalyst, 0.5-2.0 parts of foam stabilizer, 3.0-4.5 parts of water, 1-20 parts of foaming agent, uniformly stirred for 10 minutes at a stirring speed of 2000-3000 rpm and a stirring temperature of 20-30° C. to obtain component A;

[0020] (2) Preparation of component B: Add 60-80 parts of toluene diisocyanate and 20-40 parts of diphenylmethane diisocyanate into a container, and stir and mix for 10 minutes to obtain material B; the stirring speed is 2000-5000 rpm, and the stirring temperature is 20-30° C.;

[0021] (3) Component A and component B are poured into a mold in a weight percentage of 100:40-70 by a high-pressure or low-pressure foaming machine, and the mold is opened for 3-6 minutes and taken out from the mold to obtain a product.

[0022] To solve the third of the above technical problems, the technical solution adopted by the present invention is as follows: a low-density, high-comfort polyurethane foam plastic can be applied to car seats.

[0023] The low-density, high-comfort polyurethane foam plastic of the present invention comprises a polyether polyol A1 having a molecular weight of 6000-10000, a functionality of 2-4, an unsaturation of less than 0.04 mol / kg, and a primary hydroxyl content of more than 85%; a Mannich polyether polyol A2 having a functionality of 3, a hydroxyl value of 240-390 mgKOH / g; a polymer polyol A3 having a functionality of 3, a hydroxyl value of 15-28 mgKOH / g, and a solid content of 27-47%; a crosslinking agent, an amine reaction catalyst, a low-atomization silicone oil, water, and a foaming agent to form component A; and component B being a mixture of toluene diisocyanate and diphenylmethane diisocyanate having an isocyanate content of 37.2-47.5%. The inventor surprisingly found that a high-resilience polyurethane foam plastic with low density and low hysteresis loss is obtained by the reaction of component A and component B. The polyurethane foam plastic has not only a low density (35.2-44.8 kg / m 3), and the hysteresis loss is also lower (15.2-16.7%), and the vibration transmittance is lower at around 5Hz, which improves the comfort of the product and achieves better technical results. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is the resonance frequency curve of the low-density, high-comfort polyurethane foam plastics prepared in Comparative Example 1 and Example 8. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with specific embodiments. The described embodiments are only a part of the embodiments of the present invention, but not all of the embodiments.

[0026] Table 2 List of raw materials

[0027]

[0028]

[0029]

[0030] Example 1

[0031] (1) Preparation of component A

[0032] In parts by weight, 88 parts of polyether polyol A1.1, 2 parts of Mannich polyether polyol A2.1, 10 parts of polymer polyol A3.1, 0.85 parts of diethanolamine, 0.05 parts of ZF-10, 0.63 parts of Z-130, 0.62 parts of B-8734, 3.6 parts of water, and 3.0 parts of foaming agent were added into container A in sequence, and stirred for 10 minutes to prepare component A;

[0033] (2) Preparation of component B

[0034] In container B, add 60 parts of T-80 and 40 parts of polymeric MDI M20S according to weight parts, and stir for 10 minutes to obtain component B with an isocyanate mass percentage of 41.2%;

[0035] (3) Component A and component B in a weight ratio of 100:47 are poured into a mold through a high-pressure foaming machine, and the reaction is carried out in a mold heated by a water bath at a mold temperature of 65° C. The mold is opened after 4.5 minutes and taken out from the mold to obtain a low-density, low-hysteresis polyurethane foam.

[0036] Embodiments 2 to 8

[0037] Examples 2 to 8 are carried out according to the steps in Example 1, except that the reaction raw materials, raw material ratios, and demolding times are different, as shown in Table 3.

[0038] Table 3 Weight parts of each component raw material in Examples 1 to 8

[0039]

[0040]

[0041]

[0042] Comparative Examples 1 to 3

[0043] Comparative Examples 1 to 3 were carried out according to the steps in Example 1, except that the reaction raw materials, raw material ratios, and demolding time were different, as shown in Table 4. The performance index data of the low-density, high-comfort polyurethane foam plastics obtained are shown in Table 5. The resonance frequency curve of the low-density, high-comfort polyurethane foam plastics obtained is shown in Table 6. Figure 1 shown.

[0044] Table 4 Weight parts of each component raw material in Comparative Examples 1 to 3

[0045]

[0046]

[0047] Table 5 Performance test data of low-density, high-comfort polyurethane foams prepared in Examples 1 to 8 and Comparative Examples 1 to 4

[0048]

[0049]

[0050] From the comparison of Table 3 and Table 4, it can be seen that in Examples 1 to 8 of the present invention, a high-activity polyether with a functionality greater than 3, a molecular weight of 6000 to 12000, and a primary hydroxyl mass percentage of greater than 85% and a Mannich polyether polyol A2 with a functionality of 3 and a hydroxyl value of 240 to 390 mgKOH / g are used for formulation development, and the demoulding time of the foam plastic is 3.2 to 4.5 min, which is better than that of Comparative Examples 1 to 4 (4.5 to 5.3 min); From Table 5, it can be seen that the foaming agent selected by the present invention is used for formulation development, so that the density of the polyurethane foam (35.2 to 44.8 kg / m 3 )Compared to 1~4(45~55kg / m 3 ) is lower. After the density is reduced, the resilience (60%-65%), 40% compression strength (6.2-7.8 kPa), hysteresis loss (15.2-16.7%) and odor level (2.5-3.0) of the polyurethane foam plastic can still meet all the requirements of car seats.

[0051] By the attached Figure 1It can be seen that the foam plastic made from high-activity polyether with a functionality greater than 3, a molecular weight of 6000-12000, and a primary hydroxyl mass percentage greater than 85% in Example 8 of the present invention does not significantly increase the transmittance above 5 Hz when the product thickness is reduced to 8 cm (that is, the density is also reduced), thereby ensuring the comfort of the product and can be used in industrial applications of automotive interior seats.

Claims

1. A low-density, high-comfort polyurethane foam plastic comprising: The invention is composed of component A and component B, wherein the weight percentage of component A to component B is 100:40-70, wherein component A comprises the following components in parts by weight: 40-100 parts of polyether polyol A1, 0-30 parts of Mannich polyether polyol A2, 0-30 parts of polymer polyol A3, 0.1-1.0 parts of crosslinking agent, 0.1-1.0 parts of amine reaction catalyst, 0.5-2.0 parts of foam stabilizer, 3.0-4.5 parts of water and 1-20 parts of foaming agent; component B is various multifunctional aliphatic, alicyclic and aromatic isocyanates. The polyether polyol A1 is prepared by polymerization of active hydrogen compounds and olefin oxides using organic phosphorus alcohol salts as catalysts, and has a molecular weight of 4000-15000, a functionality of 2-6, a molecular weight distribution coefficient of 1.0-1.06, an unsaturation of ≤0.04 mmol / g, and a primary hydroxyl content of more than 85%. The Mannich polyether polyol A2 is gradually synthesized by Mannich reaction, has an aromatic ring structure, a hydroxyl value of 240-390 mgKOH / g, and a functionality of 2-4. The polymer polyol A3 has a hydroxyl value of 15-28 mgKOH / g, a functionality of 2-4, and a solid content of 27-47%.

2. The low-density, high-comfort polyurethane foam plastic according to claim 1, characterized in that: The active hydrogen compound of the polyether polyol A1 in component A is an organic compound containing hydroxyl groups, selected from hydroxy alcohols, sugars or their derivatives having 2 to 20 carbon atoms and 1 to 8 hydroxyl groups, or polyether polyols having 2 to 8 hydroxyl groups and a number average molecular weight of 200 to 5000; the oxidized olefin is selected from at least one of ethylene oxide, propylene oxide, 1,2-butylene oxide or styrene oxide.

3. The low-density, high-comfort polyurethane foam plastic according to claim 1, characterized in that: The molecular weight of the polyether polyol A1 in component A is 6000-10000 and the functionality is 2-4.

4. The low-density, high-comfort polyurethane foam plastic according to claim 1, characterized in that: The crosslinking agent in component A is selected from one or a combination of diethanolamine and triethanolamine; the amine reaction catalyst is selected from one or a combination of ZF-10, Z-130, DMEA, and NE-1070; the foam stabilizer is selected from one or a combination of low-atomization B-8734, B-8738, and B-8715.

5. The low-density, high-comfort polyurethane foam plastic according to claim 1, characterized in that: The foaming agent in component A is selected from one or a combination of 245FA and LBA. Due to the particularity of these two components, the foaming agent has little harm to the human body and is very friendly to the environment.

6. The low-density, high-comfort polyurethane foam plastic according to claim 1, characterized in that: Component B is selected from one or a combination of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), xylene diisocyanate, and polymethylene polyphenylene polyisocyanate.

7. A method for preparing a low-density, high-comfort polyurethane foam plastic according to claim 1, comprising the following steps: (1) Preparation of component A: In a container, according to weight parts, 140-100 parts of polyether polyol A, 20-30 parts of Mannich polyether polyol A, 30-30 parts of polymer polyol A, 0.1-1.0 parts of crosslinking agent, 0.1-1.0 parts of amine reaction catalyst, 0.5-2.0 parts of foam stabilizer, 3.0-4.5 parts of water, 1-20 parts of foaming agent, uniformly stirred for 10 minutes at a stirring speed of 2000-3000 rpm and a stirring temperature of 20-30° C. to obtain component A; (2) Preparation of component B: Add 60-80 parts of toluene diisocyanate and 20-40 parts of diphenylmethane diisocyanate into a container, and stir and mix for 10 minutes to obtain material B; the stirring speed is 2000-5000 rpm, and the stirring temperature is 20-30° C.; (3) Component A and component B are poured into a mold in a weight percentage of 100:40-70 by a high-pressure or low-pressure foaming machine, and the mold is opened for 3-6 minutes and taken out from the mold to obtain a product.

8. The method for preparing a low-density, high-comfort polyurethane foam plastic according to claim 7, characterized in that: The reaction is matured in an aluminum mold, the mold temperature is 50-70°C, the maturation time is 3-6 minutes, and the mold is demoulded. The density of the molded product is 35-45 kg / m 3 .

9. Use of the low-density, high-comfort polyurethane foam plastic according to claim 1 in automobile seats.