Polyurethane-polyacrylate composite emulsion as well as preparation method and application thereof

Through the preparation of polyurethane-polyacrylate composite emulsion, the cross-linking reaction between ketone and hydrazine groups was used to solve the problems of low temperature resistance, bonding strength and water resistance of printing glue in the prior art, and achieve a higher Comprehensive performance and convenience of use.

CN118930803APending Publication Date: 2024-11-12DONGGUAN CTL NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174130.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing acrylate coatings and polyurethane emulsions have problems such as low temperature resistance, hot viscosity, cold brittleness and insufficient bonding strength in printing glue. The polyurethane emulsion has poor water resistance, high price, and is not widely used.

Method used

The polyurethane-polyacrylate composite emulsion is adopted to achieve cross-linking through the introduction of ketone groups and hydrazine groups, and the dehydration and condensation reaction is carried out, combining the advantages of polyacrylates and aqueous polyurethane emulsions to enhance the comprehensive performance of the printing glue.

Benefits of technology

It significantly improves the comprehensive performance of printing glue, including improving its stretchability, friction color fastness, washing fastness and softness of the hand, and is suitable for the preparation of high-end printing glue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010229560000251
    Figure BDA0005010229560000251
  • Figure BDA0005010229560000261
    Figure BDA0005010229560000261
  • Figure BDA0005010229560000271
    Figure BDA0005010229560000271
Patent Text Reader

Abstract

The invention relates to a polyurethane-polyacrylate composite emulsion as well as a preparation method and application thereof. The preparation raw materials of the polyurethane-polyacrylate composite emulsion comprise a combination of a hydrazino-containing polyurethane emulsion and a keto-containing polyacrylate emulsion, the molar ratio of the hydrazino group in the hydrazino group-containing polyurethane emulsion to the keto group in the keto group-containing polyacrylate emulsion is (0.25 to 2): 1; the hydrazino-containing polyurethane emulsion is prepared from the following raw materials in parts by weight: 150 to 400 parts by weight of polyol, 60 to 180 parts by weight of polyisocyanate, 7 to 16 parts by weight of a hydrophilic chain extender, 10 to 30 parts by weight of a micromolecular chain extender and 5 to 15 parts by weight of a hydrazino-containing end-capping reagent. According to the polyurethane-polyacrylate composite emulsion provided by the invention, the dehydration condensation reaction between a ketone group and a hydrazine group is utilized, cross-linking of two polymers is realized during drying and film forming, the polyurethane-polyacrylate composite emulsion is used in printing rubber cement, the comprehensive performance of the printing rubber cement can be improved, and the polyurethane-polyacrylate composite emulsion is convenient to use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to a polyurethane-polyacrylate composite emulsion and a preparation method and application thereof. Background Art

[0002] Acrylate copolymer (PA) emulsion is an environmentally friendly material with good water resistance and alkali resistance. It has high gloss, strong adhesion, good powder dispersion and wetting, and is economical. It has always been the preferred emulsion for preparing general-purpose printing paste and is widely used in the fields of coatings and adhesives. CN109023999A discloses a self-cross-linking acrylic paint printing adhesive, but this type of acrylic paint generally has the disadvantages of being not resistant to low temperatures, being hot-sticky and cold-brittle, and having insufficient bonding strength.

[0003] Polyurethane (PU) emulsion has excellent adhesion to various materials, and the film has excellent elasticity, wear resistance and low temperature resistance, and has good hand feel and good weather resistance. However, due to the presence of hydrophilic groups in the molecular chain, the formed coating has poor water resistance, the price is also expensive, and it needs to add a curing agent to make it into a two-component for use, so it is generally used to prepare higher-end printing paste, and the usage is not large. Water-based polyurethane has excellent adhesion, elasticity, wear resistance and breathable and moisture permeability, but due to the presence of hydrophilic groups in the molecular chain, the formed coating has poor water resistance.

[0004] Therefore, it is urgent to develop a composite emulsion that has the advantages of both acrylic copolymer emulsion and polyurethane emulsion and is easy to use to improve the comprehensive performance of printing paste. Summary of the invention

[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a polyurethane-polyacrylate composite emulsion and a preparation method and application thereof. The polyurethane-polyacrylate composite emulsion provided by the present invention can significantly improve the comprehensive performance of the polyurethane-polyacrylate composite emulsion through the complementarity of the performance of polyacrylate emulsion and polyurethane emulsion.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a polyurethane-polyacrylate composite emulsion, wherein the raw materials for preparing the polyurethane-polyacrylate composite emulsion include a combination of a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is (0.25-2):1; in parts by weight, the raw materials for preparing the hydrazine-containing polyurethane emulsion include 150-400 parts by weight of a polyol, 60-180 parts by weight of a polyisocyanate, 7-16 parts by weight of a hydrophilic chain extender, 10-30 parts by weight of a small molecule chain extender, and 5-15 parts by weight of a hydrazine-containing end-capping agent.

[0008] The polyurethane-polyacrylate composite emulsion provided by the present invention is obtained by introducing ketone groups and hydrazine groups into polyacrylate and polyurethane molecules respectively, compounding a polyurethane emulsion containing hydrazine groups and a polyacrylate emulsion containing ketone groups according to a molar ratio of hydrazine groups to ketone groups of (0.25-2):1, utilizing the dehydration condensation reaction between ketone groups and hydrazine groups, realizing crosslinking of the two polymers during drying and film formation by a film-forming crosslinking method, combining the respective advantages of polyacrylate emulsion and aqueous polyurethane emulsion, and improving the comprehensive performance of the polyurethane-polyacrylate composite emulsion in printing.

[0009] The molar ratio of the hydrazine group in the hydrazine group-containing polyurethane emulsion to the ketone group in the ketone group-containing polyacrylate emulsion is (0.25-2):1, for example, it can be 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, etc.

[0010] The polyol is 150-400 parts by weight, for example, 150 parts by weight, 180 parts by weight, 200 parts by weight, 220 parts by weight, 250 parts by weight, 280 parts by weight, 300 parts by weight, 320 parts by weight, 350 parts by weight, 380 parts by weight, 400 parts by weight, etc.

[0011] The polyisocyanate is 60-180 parts by weight, for example, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight, 150 parts by weight, 160 parts by weight, 170 parts by weight, 180 parts by weight, etc.

[0012] The hydrophilic chain extender is 7-16 parts by weight, for example, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, etc.

[0013] The small molecule chain extender is 10-30 parts by weight, for example, 10 parts by weight, 12 parts by weight, 14 parts by weight, 16 parts by weight, 18 parts by weight, 20 parts by weight, 22 parts by weight, 24 parts by weight, 26 parts by weight, 28 parts by weight, etc.

[0014] The hydrazine-containing end-capping agent is 5-15 parts by weight, for example, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, etc.

[0015] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0016] As a preferred technical solution, the number average molecular weight of the polyol is 600-3000, for example, 600, 800, 1000, 1200, 1400, 1600, 1800, 2000, 2200, 2400, 2600, 2800, 3000, etc.

[0017] Preferably, the polyol includes any one or a combination of at least two of polycaprolactone diol, polycarbonate diol, polypropylene glycol, polytetramethylene glycol, polybutylene adipate or castor oil.

[0018] Preferably, the polyisocyanate includes any one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate or hexamethylene diisocyanate, or a combination of at least two thereof.

[0019] Preferably, the hydrophilic chain extender comprises a carboxylic acid type hydrophilic chain extender.

[0020] Preferably, the carboxylic acid type hydrophilic chain extender comprises 2,2-dimethylol propionic acid and / or 2,2-dimethylol butyric acid.

[0021] Preferably, the small molecule chain extender includes a polyamine chain extender.

[0022] Preferably, the polyamine chain extender includes any one of isophoronediamine, ethylenediamine or diethylenetriamine, or a combination of at least two thereof.

[0023] Preferably, the hydrazine-containing end-capping agent includes any one of adipic acid dihydrazide, oxalic acid dihydrazide, carbonate dihydrazide or succinic acid dihydrazide, or a combination of at least two thereof, and adipic acid dihydrazide and / or oxalic acid dihydrazide are further preferred.

[0024] Preferably, the raw materials for preparing the hydrazine-containing polyurethane emulsion further include 7-16 parts by weight of a first neutralizer, 30-150 parts by weight of an organic solvent and 400-500 parts by weight of water.

[0025] The first neutralizer is 7-16 parts by weight, for example, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, etc.

[0026] The organic solvent is 30-150 parts by weight, for example, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight, 150 parts by weight, etc.

[0027] The water is 400-500 parts by weight, for example, 410 parts by weight, 420 parts by weight, 430 parts by weight, 440 parts by weight, 450 parts by weight, 460 parts by weight, 470 parts by weight, 480 parts by weight, 490 parts by weight, 500 parts by weight, etc.

[0028] Preferably, the first neutralizing agent comprises triethylamine and / or triethanolamine.

[0029] Preferably, the organic solvent comprises acetone and / or dimethylformamide.

[0030] Preferably, the raw materials for preparing the hydrazine-containing polyurethane emulsion further include a catalyst.

[0031] Preferably, the catalyst comprises an organobismuth catalyst.

[0032] Preferably, based on 100% of the mass of the hydrazine-containing polyurethane emulsion, the mass of the catalyst is 0.1-1%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc.

[0033] Preferably, the method for preparing the hydrazine-containing polyurethane emulsion comprises the following steps:

[0034] (F1) reacting the polyol, the polyisocyanate and the hydrophilic chain extender to obtain a polyurethane prepolymer;

[0035] (F2) mixing the polyurethane prepolymer with water for emulsification dispersion, adding the small molecule chain extender for a first reaction during and / or after the emulsification dispersion, and then adding the hydrazine-containing end-capping agent for a second reaction to obtain the hydrazine-containing polyurethane emulsion.

[0036] Preferably, the reaction in step (F1) is carried out in the presence of the catalyst.

[0037] Preferably, the reaction in step (F1) is carried out according to the following steps:

[0038] (M1) pre-reacting the polyol with the polyisocyanate to obtain a first reaction system;

[0039] (M2) the first reaction system reacts with the hydrophilic chain extender to obtain a second reaction system;

[0040] (M3) The second reaction system reacts with the catalyst to obtain the polyurethane prepolymer.

[0041] Preferably, the temperature of the pre-reaction is 80-120°C, for example, it can be 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C, 120°C, etc.

[0042] Preferably, the pre-reaction time is 2-5 h, for example, it can be 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h, 4 h, 4.2 h, 4.4 h, 4.6 h, 4.8 h, 5 h, etc.

[0043] Preferably, the reaction temperature in step (M2) is 40-80°C, for example, it can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 55°C, 58°C, 60°C, 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, etc.

[0044] Preferably, the reaction time of step (M2) is 1-3 h, for example, it can be 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, etc.

[0045] Preferably, the reaction temperature in step (M3) is 40-80°C, for example, it can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 55°C, 58°C, 60°C, 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, etc.

[0046] Preferably, the reaction time of step (M3) is 4-5 h, for example, it can be 4 h, 4.1 h, 4.2 h, 4.3 h, 4.4 h, 4.5 h, 4.6 h, 4.7 h, 4.8 h, 4.9 h, 5 h, etc.

[0047] Preferably, the emulsification dispersion temperature is 10-40°C, for example, it can be 10°C, 12°C, 15°C, 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, 32°C, 35°C, 38°C, 40°C, etc.

[0048] Preferably, the emulsification and dispersion time is 10-120 min, for example, it can be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, etc.

[0049] Preferably, the emulsification dispersion is performed in the presence of the organic solvent.

[0050] Preferably, before the mixing in step (F2), the step further includes the step of neutralizing the polyurethane prepolymer using the first neutralizing agent.

[0051] Preferably, the neutralization temperature is 30-50°C, for example, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, etc.

[0052] Preferably, the neutralization time is 10-15 min, for example, it can be 10 min, 10.5 min, 11 min, 11.5 min, 12 min, 12.5 min, 13 min, 13.5 min, 14 min, 14.5 min, 15 min, etc.

[0053] Preferably, the temperature of the first reaction is 10-30°C, for example, it can be 10°C, 12°C, 15°C, 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, etc.

[0054] Preferably, the time of the first reaction is 20-60 min, for example, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0055] Preferably, the temperature of the second reaction is 10-30°C, for example, 10°C, 12°C, 15°C, 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, etc.

[0056] Preferably, the time of the second reaction is 30-60 min, for example, it can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0057] Preferably, after the second reaction is completed, the method further comprises the step of removing the organic solvent.

[0058] Preferably, the raw materials for preparing the ketone-containing polyacrylate emulsion include polymerizable monomers; in parts by weight, the polymerizable monomers include 45-150 parts by weight of hard monomers, 150-400 parts by weight of soft monomers and 5-10 parts by weight of ketone-containing functional monomers.

[0059] The hard monomer is 45-150 parts by weight, for example, 45 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight, 150 parts by weight, etc.

[0060] The soft monomer is 150-400 parts by weight, for example, 150 parts by weight, 180 parts by weight, 200 parts by weight, 220 parts by weight, 250 parts by weight, 280 parts by weight, 300 parts by weight, 320 parts by weight, 350 parts by weight, 380 parts by weight, 400 parts by weight, etc.

[0061] The ketone group-containing functional monomer is 5-10 parts by weight, for example, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, etc.

[0062] Preferably, the hard monomer includes any one of methyl methacrylate, styrene or acrylonitrile, or a combination of at least two thereof.

[0063] Preferably, the soft monomer includes any one of ethyl acrylate, n-butyl acrylate or isooctyl acrylate, or a combination of at least two of them.

[0064] Preferably, the ketone group-containing functional monomer includes diacetone acrylamide and / or ethyl acetoacetate methacrylate.

[0065] Preferably, the polymerizable monomer further comprises a first functional monomer; the first functional monomer comprises any one or a combination of at least two of hydroxyethyl acrylate, acrylic acid, itaconic acid or methacrylic acid.

[0066] Preferably, in parts by weight, the first functional monomer is 5-10 parts by weight, for example, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, etc.

[0067] Preferably, the total mass percentage of the ketone-containing functional monomer and the first functional monomer in the polymerizable monomer is 2-8%, for example, 2.5%, 3.5%, 4.5%, 5.5%, 6.5%, 7.5%, 8%, etc.

[0068] Preferably, the mass percentage of the hard monomer in the polymerized monomer is 10-45%, for example, it can be 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, etc.

[0069] Preferably, the mass percentage of the soft monomer in the polymerized monomer is 50-84%, for example, it can be 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72%, 75%, 78%, 80%, 82%, 84%, etc.

[0070] Preferably, in parts by weight, the raw materials for preparing the ketone-containing polyacrylate emulsion also include 200-400 parts by weight of water, 1-15 parts by weight of anionic emulsifier, 0.5-5.5 parts by weight of nonionic emulsifier, 1.5-3.5 parts by weight of initiator, 0.1-1.5 parts by weight of buffer and 1-10 parts by weight of second neutralizer.

[0071] The water is 200-400 parts by weight, for example, 200 parts by weight, 220 parts by weight, 240 parts by weight, 260 parts by weight, 280 parts by weight, 300 parts by weight, 320 parts by weight, 340 parts by weight, 360 parts by weight, 380 parts by weight, 400 parts by weight, etc.

[0072] The anionic emulsifier is 1-15 parts by weight, for example, it can be 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, etc.

[0073] The nonionic emulsifier is 0.5-5.5 parts by weight, for example, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, etc.

[0074] The initiator is 1.5-3.5 parts by weight, for example, 1.5 parts by weight, 1.8 parts by weight, 2 parts by weight, 2.2 parts by weight, 2.5 parts by weight, 2.8 parts by weight, 3 parts by weight, 3.2 parts by weight, 3.5 parts by weight, etc.

[0075] The buffer is 0.1-1.5 parts by weight, for example, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, etc.

[0076] The second neutralizer is 1-10 parts by weight, for example, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, etc.

[0077] Preferably, the anionic emulsifier comprises sodium dodecyl sulfate and / or sodium dodecylbenzene sulfonate.

[0078] Preferably, the nonionic emulsifier comprises fatty alcohol polyoxyethylene ether.

[0079] Preferably, the initiator comprises ammonium persulfate.

[0080] Preferably, the initiator is dissolved in water and used in the form of an initiator aqueous solution.

[0081] Preferably, the mass percentage of the initiator in the initiator aqueous solution is 0.2-5%, for example, it can be 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, etc.

[0082] Preferably, the buffer comprises any one of disodium hydrogen phosphate, sodium bicarbonate or potassium hydroxide, or a combination of at least two thereof.

[0083] Preferably, the second neutralizing agent comprises aqueous ammonia.

[0084] Preferably, the method for preparing the ketone-containing polyacrylate emulsion comprises the following steps:

[0085] (S1) mixing the hard monomer, the soft monomer, optionally the first functional monomer, water, the anionic emulsifier and the nonionic emulsifier to obtain a pre-emulsion; the pre-emulsion is divided into a first pre-emulsion, a second pre-emulsion and a third pre-emulsion;

[0086] (S2) mixing the first pre-emulsion with water and performing a third reaction to obtain a seed emulsion;

[0087] (S3) After the seed emulsion and the second pre-emulsion undergo a fourth reaction, the fourth pre-emulsion is added to sequentially undergo a fifth reaction and heat preservation to obtain the ketone-containing polyacrylate emulsion; the fourth pre-emulsion is composed of the third pre-emulsion and the ketone-containing functional monomer.

[0088] In the present invention, the pre-emulsion prepared in step (S1) needs to be divided into three parts, namely the first pre-emulsion, the second pre-emulsion and the third pre-emulsion for subsequent steps. The compositions of these three pre-emulsions are exactly the same as the pre-emulsion, and the total mass of the three pre-emulsions is equal to the mass of the pre-emulsion.

[0089] Preferably, based on the mass of the pre-emulsion as 100%, the mass of the first pre-emulsion is 4-6% (for example, 4%, 4.2%, 4.4%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.6%, 5.8%, 6%, etc.), and the mass of the second pre-emulsion is 76-87.9% (for example, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, etc.).

[0090] Preferably, the solid content of the pre-emulsion is 45-90%, for example, it can be 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90% and the like; further preferably, it is 70-80%, for example, it can be 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% and the like.

[0091] Preferably, the temperature of the third reaction is 50-70°C, for example, 50°C, 52°C, 55°C, 58°C, 60°C, 62°C, 65°C, 68°C, 70°C, etc.

[0092] Preferably, the time of the third reaction is 0.1-1 h, for example, it can be 0.1 h, 0.2 h, 0.3 h, 0.4 h, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, etc.

[0093] Preferably, the mixed material in step (S2) further includes the buffer.

[0094] Preferably, the third reaction, the fourth reaction and the fifth reaction are all carried out in the presence of the initiator.

[0095] Preferably, the mass ratio of the initiators used in the third reaction, the fourth reaction and the fifth reaction is 1:(2-4):(1-2), for example, 1:2.2:1.05, 1:2.4:1.1, 1:2.6:1.15, 1:2.8:1.2, 1:3:1.25, 1:3.2:1.3, 1:3.4:1.35, 1:3.6:1.4, 1:3.8:1.45, 1:4:1.5, 1:4:1.6, 1:4:1.7, 1:4:1.8, 1:4:1.9, etc.

[0096] Preferably, the temperature of the fourth reaction is 70-85°C, for example, it can be 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, etc.

[0097] Preferably, the fourth reaction time is 2-4 h, for example, it can be 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h, 4 h, etc.

[0098] Preferably, the second pre-emulsion and the initiator are added to the reaction system in a dropwise manner.

[0099] Preferably, the temperature of the fifth reaction is 70-85°C, for example, it can be 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, etc.

[0100] Preferably, the time of the fifth reaction is 0.5-2 h, for example, it can be 0.5 h, 0.6 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, etc.

[0101] Preferably, the fourth pre-emulsion and the initiator are added to the reaction system in a dropwise manner.

[0102] Preferably, the insulation temperature is 80-82°C, for example, it can be 80°C, 80.2°C, 80.4°C, 80.6°C, 80.8°C, 81°C, 81.2°C, 81.4°C, 81.6°C, 81.8°C, 82°C, etc.

[0103] Preferably, the insulation time is 1-3 h, for example, it can be 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, etc.

[0104] Preferably, after the insulation is completed, the step of adding the second neutralizing agent is also included.

[0105] Preferably, the raw materials for preparing the polyurethane-polyacrylate composite emulsion also include a first defoaming agent.

[0106] Preferably, the first defoaming agent comprises a polysiloxane defoaming agent and / or a mineral oil defoaming agent.

[0107] Preferably, the mass percentage of the first defoamer in the polyurethane-polyacrylate composite emulsion is 0.2-1%, for example, it can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc.

[0108] In a second aspect, the present invention provides a method for preparing the polyurethane-polyacrylate composite emulsion as described in the first aspect, the preparation method comprising:

[0109] The polyurethane emulsion containing hydrazine groups is mixed with the polyacrylate emulsion containing ketone groups to obtain the polyurethane-polyacrylate composite emulsion.

[0110] Preferably, the mixed material further comprises a first defoaming agent.

[0111] In a third aspect, the present invention provides a printing paste, which comprises the following components, in parts by weight: 50-100 parts by weight of the polyurethane-polyacrylate composite emulsion as described in the first aspect, 5-15 parts by weight of a moisturizer, 0.5-1 parts by weight of a third neutralizer, 0.3-2 parts by weight of an emulsifier, 0.1-1 parts by weight of a second defoaming agent, 1-5 parts by weight of a softener and 1-3 parts by weight of a thickener.

[0112] The polyurethane-polyacrylate composite emulsion is 50-100 parts by weight, for example, it can be 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, etc.

[0113] The moisturizer is 5-15 parts by weight, for example, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, etc.

[0114] The third neutralizer is 0.5-1 parts by weight, for example, 0.5 parts by weight, 0.55 parts by weight, 0.6 parts by weight, 0.65 parts by weight, 0.7 parts by weight, 0.75 parts by weight, 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight, 0.95 parts by weight, 1 part by weight, etc.

[0115] The emulsifier is 0.3-2 parts by weight, for example, 0.3 parts by weight, 0.4 parts by weight, 0.6 parts by weight, 0.8 parts by weight, 1 part by weight, 1.2 parts by weight, 1.4 parts by weight, 1.6 parts by weight, 1.8 parts by weight, 2 parts by weight, etc.

[0116] The second defoaming agent is 0.1-1 parts by weight, for example, it can be 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.55 parts by weight, 0.6 parts by weight, 0.65 parts by weight, 0.7 parts by weight, 0.75 parts by weight, 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight, 0.95 parts by weight, 1 part by weight, etc.

[0117] The softener is 1-5 parts by weight, for example, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, etc.

[0118] The thickener is 1-3 parts by weight, for example, 1 part by weight, 1.2 parts by weight, 1.5 parts by weight, 1.8 parts by weight, 2 parts by weight, 2.2 parts by weight, 2.5 parts by weight, 2.8 parts by weight, or 3 parts by weight.

[0119] Preferably, the humectant comprises glycerin and / or propylene glycol.

[0120] Preferably, the third neutralizing agent includes any one of triethanolamine, diethanolamine or triethylamine, or a combination of at least two of them.

[0121] Preferably, the emulsifier comprises isomeric tridecanol polyoxyethylene ether and / or primary alcohol polyoxyethylene ether.

[0122] Preferably, the second defoamer comprises a mineral oil defoamer and / or a silicone defoamer.

[0123] Preferably, the softener comprises diethylene glycol and / or dipropylene glycol dibenzoate.

[0124] Preferably, the thickener comprises an alkali swellable thickener and / or a polyurethane associative thickener.

[0125] Compared with the prior art, the present invention has the following beneficial effects:

[0126] (1) The polyurethane-polyacrylate composite emulsion provided by the present invention can significantly improve the comprehensive performance of the polyurethane-polyacrylate composite emulsion through the complementary performance of the polyacrylate emulsion and the polyurethane emulsion; and is easy to use and does not need to be prepared on the spot;

[0127] (2) The polyurethane-polyacrylate composite emulsion provided by the present invention is used for printing paste, which can improve its stretchability and color fastness to friction, wherein the wet rubbing color fastness can reach level 2-3, and the dry rubbing color fastness can reach level 2-4; it can also improve its washing fastness, and the appearance color change level after washing is level 2-5, the printing does not fall off, and it feels soft. DETAILED DESCRIPTION

[0128] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0129] The sources of some components in the embodiments and comparative examples are as follows:

[0130] (1) Polybutylene adipate: CMA-44 purchased from Jining Liduo Chemical Co., Ltd., with a number average molecular weight of 2000;

[0131] (2) Polytetrahydrofuran diol: P1000 purchased from Jining Liduo Chemical Co., Ltd., with a number average molecular weight of 1000;

[0132] (3) Organic bismuth catalyst 2810: Bi2810 purchased from Umicore;

[0133] (4) Fatty alcohol polyoxyethylene ether: purchased from Hai'an Petrochemical Plant, Jiangsu Province, TO 3070;

[0134] (5) Mineral oil defoamer: purchased from Shanghai Guangbai New Materials Co., Ltd., MO2190.

[0135] Example 1

[0136] A polyurethane-polyacrylate composite emulsion, wherein raw materials for preparing the polyurethane-polyacrylate composite emulsion include a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 0.25:1; in parts by weight, the raw materials for preparing the hydrazine-containing polyurethane emulsion include 160 parts by weight of poly(1,4-butylene adipate), 120 parts by weight of polytetrahydrofuran diol, 120 parts by weight of dicyclohexylmethane diisocyanate, 14 parts by weight of 2,2-dimethylol propionic acid, 16 parts by weight of isophorone diamine, 12 parts by weight of adipic acid dihydrazide, 28101.8 parts by weight of an organic bismuth catalyst, 14 parts by weight of triethylamine, 30 parts by weight of acetone and 400 parts by weight of deionized water;

[0137] The preparation method of the hydrazine-containing polyurethane emulsion comprises the following steps:

[0138] (F1) under nitrogen protection, adding the above-mentioned poly(1,4-butylene adipate), polytetrahydrofuran diol and dicyclohexylmethane diisocyanate to a reaction kettle, and pre-reacting at 90° C. for 2 h; then adding 2,2-dihydroxymethylpropionic acid and reacting at 80° C. for 3 h, cooling to 68° C., adding an organic bismuth catalyst 2810, and reacting at 70° C. for 4 h to obtain a polyurethane prepolymer;

[0139] (F2) adding triethylamine to the polyurethane prepolymer at 30° C. for neutralization for 10 minutes, adding acetone and deionized water for emulsification and dispersion for 10 minutes, adding isophorone diamine for reaction for 30 minutes, adding adipic acid dihydrazide for reaction for 30 minutes, and removing acetone under reduced pressure to obtain the hydrazine-containing polyurethane emulsion;

[0140] The preparation method of the ketone-containing polyacrylate emulsion comprises the following steps:

[0141] (S1) taking 2.5 parts by weight of sodium lauryl sulfate, 1 part by weight of fatty alcohol polyoxyethylene ether, 200 parts by weight of n-butyl acrylate, 45 parts by weight of styrene, 5 parts by weight of acrylic acid and 85 parts by weight of deionized water for pre-emulsification to obtain a pre-emulsion;

[0142] (S2) adding 155 parts by weight of deionized water and 0.5 parts by weight of sodium bicarbonate into a three-necked flask, then heating to 70° C., adding 4% by weight of the pre-emulsion into the three-necked flask, and then adding an aqueous ammonium persulfate solution prepared by 0.3 parts by weight of ammonium persulfate and 10 parts by weight of deionized water, and reacting until a faint blue light appears (reaction time 0.5 h), to obtain a seed emulsion;

[0143] (S3) at 80° C., 76% by weight of the pre-emulsion and an aqueous solution of ammonium persulfate (composed of 1 part by weight of ammonium persulfate and 20 parts by weight of deionized water) are added dropwise to the seed emulsion at a constant speed for reaction, and the dropping time is 2 hours; 5 parts by weight of ethyl acetoacetate methacrylate are added to the remaining pre-emulsion and mixed evenly, and then the pre-emulsion containing ethyl acetoacetate methacrylate and an aqueous solution of ammonium persulfate (composed of 0.5 parts by weight of ammonium persulfate and 10 parts by weight of deionized water) are added dropwise to the reaction system, and the addition is completed over 1 hour. After the addition is completed, the reaction is continued at a constant temperature for 30 minutes, and then the mixture is kept at 82° C. for 2 hours, cooled to 50° C., 4 parts by weight of aqueous ammonia are added, stirred evenly, and then discharged to obtain the ketone-containing polyacrylate emulsion;

[0144] The preparation method of the polyurethane-polyacrylate composite emulsion comprises: taking 31.59 parts by weight of the hydrazine-containing polyurethane emulsion and 118.41 parts by weight of the ketone-containing polyacrylate emulsion, physically mixing them, and then adding 0.6 parts by weight of a mineral oil defoamer to obtain the polyurethane-polyacrylate composite emulsion.

[0145] Example 2

[0146] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that 52.18 parts by weight of a hydrazine-containing polyurethane emulsion and 97.82 parts by weight of a ketone-containing polyacrylate emulsion are physically mixed, and other raw materials, amounts and preparation methods are the same as those in Example 1 to obtain the polyurethane-polyacrylate composite emulsion, wherein the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 0.5:1.

[0147] Example 3

[0148] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that 66.68 parts by weight of a hydrazine-containing polyurethane emulsion and 83.32 parts by weight of a ketone-containing polyacrylate emulsion are physically mixed, and other raw materials, amounts and preparation methods are the same as those in Example 1 to obtain the polyurethane-polyacrylate composite emulsion, and the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 0.75:1.

[0149] Example 4

[0150] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that 77.43 parts by weight of a hydrazine-containing polyurethane emulsion and 72.57 parts by weight of a ketone-containing polyacrylate emulsion are physically mixed, and other raw materials, amounts and preparation methods are the same as those in Example 1 to obtain the polyurethane-polyacrylate composite emulsion, wherein the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1:1.

[0151] Example 5

[0152] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that 87.99 parts by weight of a hydrazine-containing polyurethane emulsion and 62.01 parts by weight of a ketone-containing polyacrylate emulsion are physically mixed, and other raw materials, amounts and preparation methods are the same as those in Example 1 to obtain the polyurethane-polyacrylate composite emulsion, and the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1.33:1.

[0153] Example 6

[0154] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that 102.14 parts by weight of a hydrazine-containing polyurethane emulsion and 47.86 parts by weight of a ketone-containing polyacrylate emulsion are physically mixed, and other raw materials, amounts and preparation methods are the same as those in Example 1 to obtain the polyurethane-polyacrylate composite emulsion, and the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 2:1.

[0155] Example 7

[0156] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 4 only in that 12 parts by weight of adipic acid dihydrazide in the raw materials for preparing the hydrazine group-containing polyurethane emulsion are replaced with 8 parts by weight of oxalic acid dihydrazide, and other raw materials, amounts and preparation methods are the same as those in Example 4, to obtain the polyurethane-polyacrylate composite emulsion, wherein the molar ratio of the hydrazine group in the hydrazine group-containing polyurethane emulsion to the ketone group in the ketone group-containing polyacrylate emulsion is 1:1.

[0157] Example 8

[0158] A polyurethane-polyacrylate composite emulsion, wherein raw materials for preparing the polyurethane-polyacrylate composite emulsion include a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1:1; in parts by weight, the raw materials for preparing the hydrazine-containing polyurethane emulsion include 160 parts by weight of poly(1,4-butylene adipate), 120 parts by weight of polytetrahydrofuran diol, 120 parts by weight of dicyclohexylmethane diisocyanate, 16 parts by weight of 2,2-dimethylol propionic acid, 14 parts by weight of isophorone diamine, 5 parts by weight of adipic acid dihydrazide, 28101.8 parts by weight of an organic bismuth catalyst, 16 parts by weight of triethylamine, 60 parts by weight of acetone and 400 parts by weight of deionized water;

[0159] The preparation method of the hydrazine-containing polyurethane emulsion comprises the following steps:

[0160] (F1) under nitrogen protection, adding the above-mentioned poly(1,4-butylene adipate), polytetrahydrofuran diol and dicyclohexylmethane diisocyanate to a reaction kettle, and pre-reacting at 90° C. for 3 h; then adding 2,2-dihydroxymethylpropionic acid and reacting at 80° C. for 3 h, cooling to 68° C., adding an organic bismuth catalyst 2810, and reacting at 80° C. for 4 h to obtain a polyurethane prepolymer;

[0161] (F2) adding triethylamine to the polyurethane prepolymer at 30° C. for neutralization for 10 minutes, adding acetone and deionized water for emulsification and dispersion for 10 minutes, adding isophorone diamine for reaction for 30 minutes, adding adipic acid dihydrazide for reaction for 1 hour, and removing acetone under reduced pressure to obtain the hydrazine-containing polyurethane emulsion;

[0162] The preparation method of the ketone-containing polyacrylate emulsion comprises the following steps:

[0163] (S1) taking 2.5 parts by weight of sodium lauryl sulfate, 1 part by weight of fatty alcohol polyoxyethylene ether, 200 parts by weight of n-butyl acrylate, 25 parts by weight of styrene, 20 parts by weight of methyl methacrylate, 5 parts by weight of acrylic acid and 85 parts by weight of deionized water for pre-emulsification to obtain a pre-emulsion;

[0164] (S2) adding 155 parts by weight of deionized water and 0.8 parts by weight of disodium hydrogen phosphate into a three-necked flask, then heating to 70° C., adding 4% by weight of the pre-emulsion into the three-necked flask, and then adding an aqueous ammonium persulfate solution consisting of 0.3 parts by weight of ammonium persulfate and 10 parts by weight of deionized water, and reacting until a faint blue light appears (reaction time 0.5 h), to obtain a seed emulsion;

[0165] (S3) at 80° C., 76% by weight of the pre-emulsion and an aqueous solution of ammonium persulfate (composed of 1 part by weight of ammonium persulfate and 20 parts by weight of deionized water) are added dropwise to the seed emulsion at a constant speed for reaction, and the dropping time is 2 hours; 5 parts by weight of ethyl acetoacetate methacrylate are added to the remaining pre-emulsion and mixed evenly, and then the pre-emulsion containing ethyl acetoacetate methacrylate and an aqueous solution of ammonium persulfate (composed of 0.5 parts by weight of ammonium persulfate and 10 parts by weight of deionized water) are added dropwise to the reaction system, and the addition is completed over 0.5 hours. After the addition is completed, the reaction is continued at a constant temperature for 30 minutes, and then the temperature is kept at 82° C. for 1 hour, and the temperature is lowered to 50° C., 4 parts by weight of ammonia water are added, stirred evenly, and then discharged to obtain the ketone-containing polyacrylate emulsion;

[0166] The preparation method of the polyurethane-polyacrylate composite emulsion comprises: taking 107.68 parts by weight of the hydrazine-containing polyurethane emulsion and 42.32 parts by weight of the ketone-containing polyacrylate emulsion, physically mixing them, and then adding 0.6 parts by weight of a mineral oil defoamer to obtain the polyurethane-polyacrylate composite emulsion.

[0167] Example 9

[0168] A polyurethane-polyacrylate composite emulsion, wherein raw materials for preparing the polyurethane-polyacrylate composite emulsion include a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1:1; in parts by weight, the raw materials for preparing the hydrazine-containing polyurethane emulsion include 160 parts by weight of poly(1,4-butylene adipate), 120 parts by weight of polytetrahydrofuran diol, 120 parts by weight of dicyclohexylmethane diisocyanate, 14 parts by weight of 2,2-dihydroxymethylbutyric acid, 16 parts by weight of isophorone diamine, 15 parts by weight of adipic acid dihydrazide, 28102 parts by weight of an organic bismuth catalyst, 14 parts by weight of triethanolamine, 30 parts by weight of acetone and 400 parts by weight of deionized water;

[0169] The preparation method of the hydrazine-containing polyurethane emulsion comprises the following steps:

[0170] (F1) under nitrogen protection, adding the above-mentioned poly(1,4-butylene adipate), polytetrahydrofuran diol and dicyclohexylmethane diisocyanate to a reaction kettle, and pre-reacting at 90° C. for 2 h; then adding 2,2-dihydroxymethylbutyric acid and reacting at 78° C. for 2 h, cooling to 68° C., adding an organic bismuth catalyst 2810, and reacting at 70° C. for 4.5 h to obtain a polyurethane prepolymer;

[0171] (F2) adding triethanolamine to the polyurethane prepolymer at 30° C. for neutralization for 10 minutes, adding acetone and deionized water for emulsification and dispersion for 10 minutes, adding isophorone diamine for reaction for 30 minutes, adding adipic acid dihydrazide for reaction for 30 minutes, and removing acetone under reduced pressure to obtain the hydrazine-containing polyurethane emulsion;

[0172] The preparation method of the ketone-containing polyacrylate emulsion comprises the following steps:

[0173] (S1) taking 2.5 parts by weight of sodium lauryl sulfate, 1 part by weight of fatty alcohol polyoxyethylene ether, 150 parts by weight of n-butyl acrylate, 50 parts by weight of ethyl acrylate, 45 parts by weight of styrene, 5 parts by weight of acrylic acid and 85 parts by weight of deionized water for pre-emulsification to obtain a pre-emulsion;

[0174] (S2) adding 155 parts by weight of deionized water and 1 part by weight of sodium bicarbonate into a three-necked flask, then heating to 70° C., adding 4% by weight of the pre-emulsion into the three-necked flask, and then adding an aqueous ammonium persulfate solution prepared by 0.3 parts by weight of ammonium persulfate and 10 parts by weight of deionized water, and reacting until a faint blue light appears (reaction time 0.5 h), to obtain a seed emulsion;

[0175] (S3) at 80° C., 76% by weight of the pre-emulsion and an aqueous solution of ammonium persulfate (composed of 1 part by weight of ammonium persulfate and 20 parts by weight of deionized water) are added dropwise to the seed emulsion at a constant speed for reaction, and the dropping time is 2 hours; 10 parts by weight of ethyl acetoacetate methacrylate are added to the remaining pre-emulsion and mixed evenly, and then the pre-emulsion containing ethyl acetoacetate methacrylate and an aqueous solution of ammonium persulfate (composed of 0.5 parts by weight of ammonium persulfate and 10 parts by weight of deionized water) are added dropwise to the reaction system, and the addition is completed over 1.5 hours. After the addition is completed, the reaction is continued at a constant temperature for 30 minutes, and then the temperature is kept at 82° C. for 2 hours, and then the temperature is lowered to 50° C., 4 parts by weight of ammonia water are added, stirred evenly, and then discharged to obtain the ketone-containing polyacrylate emulsion;

[0176] The preparation method of the polyurethane-polyacrylate composite emulsion comprises: taking 69.18 parts by weight of the hydrazine-containing polyurethane emulsion and 80.82 parts by weight of the ketone-containing polyacrylate emulsion, physically mixing them, and then adding 0.6 parts by weight of a mineral oil defoamer to obtain the polyurethane-polyacrylate composite emulsion.

[0177] Example 10

[0178] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 4 only in that 12 parts by weight of adipic acid dihydrazide in the raw materials for preparing the hydrazine group-containing polyurethane emulsion are replaced with 10 parts by weight of succinic acid dihydrazide, and other raw materials, amounts and preparation methods are the same as those in Example 4, to obtain the polyurethane-polyacrylate composite emulsion, wherein the molar ratio of the hydrazine group in the hydrazine group-containing polyurethane emulsion to the ketone group in the ketone group-containing polyacrylate emulsion is 1:1.

[0179] Embodiment 11

[0180] A polyurethane-polyacrylate composite emulsion, wherein the raw materials for preparing the polyurethane-polyacrylate composite emulsion include a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1:1; the raw materials and preparation method of the hydrazine-containing polyurethane emulsion are the same as those in Example 4;

[0181] The preparation method of the ketone-containing polyacrylate emulsion comprises the following steps:

[0182] (S1) taking 2.5 parts by weight of sodium lauryl sulfate, 1 part by weight of fatty alcohol polyoxyethylene ether, 245 parts by weight of n-butyl acrylate, 5 parts by weight of acrylic acid and 85 parts by weight of deionized water for pre-emulsification to obtain a pre-emulsion;

[0183] (S2) adding 155 parts by weight of deionized water and 0.5 parts by weight of sodium bicarbonate into a three-necked flask, then heating to 70° C., adding 4% by weight of the pre-emulsion into the three-necked flask, and then adding an aqueous ammonium persulfate solution prepared by 0.3 parts by weight of ammonium persulfate and 10 parts by weight of deionized water, and reacting until a faint blue light appears (reaction time 0.5 h), to obtain a seed emulsion;

[0184] (S3) at 80° C., 76% by weight of the pre-emulsion and an aqueous solution of ammonium persulfate (composed of 1 part by weight of ammonium persulfate and 20 parts by weight of deionized water) are added dropwise to the seed emulsion at a constant speed for reaction, and the dropping time is 2 hours; 5 parts by weight of ethyl acetoacetate methacrylate are added to the remaining pre-emulsion and mixed evenly, and then the pre-emulsion containing ethyl acetoacetate methacrylate and an aqueous solution of ammonium persulfate (composed of 0.5 parts by weight of ammonium persulfate and 10 parts by weight of deionized water) are added dropwise to the reaction system, and the addition is completed over 1 hour. After the addition is completed, the reaction is continued at a constant temperature for 30 minutes, and then the mixture is kept at 82° C. for 2 hours, cooled to 50° C., 4 parts by weight of aqueous ammonia are added, stirred evenly, and then discharged to obtain the ketone-containing polyacrylate emulsion;

[0185] The preparation method of the polyurethane-polyacrylate composite emulsion comprises: taking 77.43 parts by weight of the hydrazine-containing polyurethane emulsion and 72.57 parts by weight of the ketone-containing polyacrylate emulsion, physically mixing them, and then adding 0.6 parts by weight of a mineral oil defoamer to obtain the polyurethane-polyacrylate composite emulsion.

[0186] Example 12

[0187] A polyurethane-polyacrylate composite emulsion, wherein the raw materials for preparing the polyurethane-polyacrylate composite emulsion include a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1:1; the raw materials and preparation method of the hydrazine-containing polyurethane emulsion are the same as those in Example 4;

[0188] The preparation method of the ketone-containing polyacrylate emulsion comprises the following steps:

[0189] (S1) taking 2.5 parts by weight of sodium lauryl sulfate, 1 part by weight of fatty alcohol polyoxyethylene ether, 200 parts by weight of n-butyl acrylate, 45 parts by weight of styrene, 5 parts by weight of acrylic acid, 5 parts by weight of ethyl acetoacetate methacrylate and 85 parts by weight of deionized water for pre-emulsification to obtain a pre-emulsion;

[0190] (S2) adding 155 parts by weight of deionized water and 0.5 parts by weight of sodium bicarbonate into a three-necked flask, then heating to 70° C., adding 4% by weight of the pre-emulsion into the three-necked flask, and then adding an aqueous ammonium persulfate solution prepared by 0.3 parts by weight of ammonium persulfate and 10 parts by weight of deionized water, and reacting until a faint blue light appears (reaction time 0.5 h), to obtain a seed emulsion;

[0191] (S3) at 80° C., 96% by weight of the pre-emulsion and an aqueous solution of ammonium persulfate (composed of 1.5 parts by weight of ammonium persulfate and 30 parts by weight of deionized water) were added dropwise to the seed emulsion at a constant speed for 3 hours, and the reaction was continued at a constant temperature for 30 minutes after the addition was completed; then, the temperature was kept at 82° C. for 2 hours, the temperature was lowered to 50° C., 4 parts by weight of aqueous ammonia were added, stirred evenly, and then discharged to obtain the ketone-containing polyacrylate emulsion;

[0192] The preparation method of the polyurethane-polyacrylate composite emulsion comprises: taking 77.43 parts by weight of the hydrazine-containing polyurethane emulsion and 72.57 parts by weight of the ketone-containing polyacrylate emulsion, physically mixing them, and then adding 0.6 parts by weight of a mineral oil defoamer to obtain the polyurethane-polyacrylate composite emulsion.

[0193] Example 13

[0194] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that in step (S1), the amount of n-butyl acrylate used is 145 parts by weight, the amount of styrene used is 100 parts by weight, and other raw materials, amounts used and preparation methods are the same as those in Example 1, to obtain the polyurethane-polyacrylate composite emulsion, wherein the molar ratio of the hydrazine group in the hydrazine group-containing polyurethane emulsion to the ketone group in the ketone group-containing polyacrylate emulsion is 0.25:1.

[0195] Comparative Example 1

[0196] A polyurethane-polyacrylate composite emulsion, wherein raw materials for preparing the polyurethane-polyacrylate composite emulsion include a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1:1; in parts by weight, the raw materials for preparing the hydrazine-containing polyurethane emulsion include 80 parts by weight of poly(1,4-butylene adipate), 60 parts by weight of polytetrahydrofuran diol, 120 parts by weight of dicyclohexylmethane diisocyanate, 14 parts by weight of 2,2-dimethylol propionic acid, 16 parts by weight of isophorone diamine, 12 parts by weight of adipic acid dihydrazide, 28101.8 parts by weight of an organic bismuth catalyst, 14 parts by weight of triethylamine, 30 parts by weight of acetone and 400 parts by weight of deionized water;

[0197] The preparation method of the hydrazine-containing polyurethane emulsion and the preparation method of the ketone-containing polyacrylate emulsion are referred to Example 4;

[0198] The preparation method of the polyurethane-polyacrylate composite emulsion comprises: physically mixing 70.75 parts by weight of the hydrazine-containing polyurethane emulsion and 79.25 parts by weight of ketone-containing polyacrylate emulsion, and then adding 0.6 parts by weight of a mineral oil defoamer to obtain the polyurethane-polyacrylate composite emulsion.

[0199] Comparative Example 2

[0200] A polyurethane-polyacrylate composite emulsion, wherein raw materials for preparing the polyurethane-polyacrylate composite emulsion include a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 1:1; in parts by weight, the raw materials for preparing the hydrazine-containing polyurethane emulsion include 240 parts by weight of poly(1,4-butylene adipate), 180 parts by weight of polytetrahydrofuran diol, 120 parts by weight of dicyclohexylmethane diisocyanate, 14 parts by weight of 2,2-dimethylol propionic acid, 16 parts by weight of isophorone diamine, 12 parts by weight of adipic acid dihydrazide, 28101.8 parts by weight of an organic bismuth catalyst, 14 parts by weight of triethylamine, 30 parts by weight of acetone and 400 parts by weight of deionized water;

[0201] The preparation method of the hydrazine-containing polyurethane emulsion and the preparation method of the ketone-containing polyacrylate emulsion are referred to Example 4;

[0202] The preparation method of the polyurethane-polyacrylate composite emulsion comprises: physically mixing 83.07 parts by weight of the hydrazine-containing polyurethane emulsion and 66.93 parts by weight of ketone-containing polyacrylate emulsion, and then adding 0.6 parts by weight of a mineral oil defoamer to obtain the polyurethane-polyacrylate composite emulsion.

[0203] Comparative Example 3

[0204] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that the hydrazine-containing polyurethane emulsion is 109.1 parts by weight, the ketone-containing polyacrylate emulsion is 40.9 parts by weight, and other raw materials, dosages and preparation methods are the same as those in Example 1, to obtain the polyurethane-polyacrylate composite emulsion, wherein the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 2.5:1.

[0205] Comparative Example 4

[0206] A polyurethane-polyacrylate composite emulsion and a preparation method thereof, which differs from Example 1 only in that the hydrazine-containing polyurethane emulsion is 26.38 parts by weight, the ketone-containing polyacrylate emulsion is 123.62 parts by weight, and other raw materials, dosages and preparation methods are the same as those in Example 1, to obtain the polyurethane-polyacrylate composite emulsion, wherein the molar ratio of the hydrazine groups in the hydrazine-containing polyurethane emulsion to the ketone groups in the ketone-containing polyacrylate emulsion is 0.2:1.

[0207] Application Example 1

[0208] A printing paste, the components of the printing paste include 80 parts by weight of the polyurethane-polyacrylate composite emulsion provided in Example 1, 10 parts by weight of glycerol, 1 part by weight of triethanolamine, 2 parts by weight of isomeric tridecanol polyoxyethylene ether (purchased from Hai'an Petrochemical Plant, Jiangsu Province, TO 3070), 1 part by weight of mineral oil defoamer (purchased from Shanghai Guangbai New Materials Co., Ltd., MO2190), 3 parts by weight of diethylene glycol and 3 parts by weight of alkali swelling thickener Dow ASE-60.

[0209] Application Example 2-13, Comparative Application Example 1-5

[0210] A printing paste, which differs from Application Example 1 only in that the polyurethane-polyacrylate composite emulsion provided in Example 1 is replaced in equal amounts by the polyurethane-polyacrylate composite emulsions provided in Examples 2-13 and Comparative Examples 1-4 and the ketone-containing polyacrylate emulsion in Example 1, and the remaining components and amounts are the same as those in Application Example 1.

[0211] Performance Testing

[0212] The printing paste provided in Application Examples 1-13 and Comparative Application Examples 1-5 was printed on high-elastic swimwear fabric to test the appearance after washing, printed on elastic fabric to test the stretchability, and printed on white cotton fabric to test the dry and wet rubbing color fastness and feel. The performance was tested according to the following method, and the test results are shown in Table 1;

[0213] (1) Washing test: According to GB / T8629-2017 "Household Washing and Drying Procedure for Textile Testing", the 4N procedure is carried out, washing 5 times, hanging to dry, and observing the discoloration level of the printed parts after washing and whether there are cracks, bubbles, peeling and shedding on the printed parts, which affect the appearance quality;

[0214] (2) Color fastness to rubbing test: According to GB / T3920-2008 Textiles - Color fastness - Tests for color fastness to rubbing, the number of rubbing is 10, and the color staining level of the rubbing cloth is evaluated;

[0215] (3) Stretchability test: Perform the stretchability test method in FZ / T70017-2022 "General Technical Requirements for Printing Quality of Knitted Garments" and observe the changes in the state of the printing after the test;

[0216] (4) Hand feel: Using the touch method, 6 laboratory personnel test and score the fabric samples, and take the average value. The printing paste is rated into 5 levels according to different hand feels. The best is level 5 and the worst is level 1. Level 5 represents very soft, level 4 represents relatively soft, level 3 represents soft, level 2 represents relatively hard, and level 1 represents hard;

[0217] Table 1

[0218]

[0219]

[0220]

[0221] It can be seen from the test data of application examples 1-9 in Table 1 that the printing glue prepared by using the polyurethane-polyacrylate composite emulsion provided by the present invention has good hand feel, good elasticity, high wet rubbing color fastness and dry rubbing color fastness, and the appearance of the water-based printing changes less. It can be seen from application examples 1-6 that when the molar ratio of the hydrazine group in the hydrazine-containing polyurethane emulsion to the ketone group in the ketone-containing polyacrylate emulsion is 1:1, the comprehensive performance of the printing glue is the best; as the content of the hydrazine group in the polyurethane-polyacrylate composite emulsion increases, the crosslinking density of the polyurethane-polyacrylate composite emulsion also gradually increases, the printing feel will gradually become harder, the adhesion of the printing glue on the white cotton cloth will improve, the dry and wet rubbing color fastness will improve, the printing will crack with the increase of the crosslinking density, and the appropriate crosslinking density can make the elasticity of the printing glue better.

[0222] From the comparison of Application Examples 4, 7 and 10, it can be seen that when succinic acid dihydrazide is used as the end-capping agent, the comprehensive performance of the printing paste becomes worse than that of oxalic acid dihydrazide and adipic acid dihydrazide.

[0223] From the comparison between Application Example 4 and Application Example 11, it can be seen that if no hard monomer is used in the preparation raw materials of the ketone-containing polyacrylate emulsion, the printing feel will become soft, the printing color fastness will deteriorate, the dry and wet rubbing color fastness will deteriorate, and the color will fade after washing.

[0224] From the comparison between Application Example 4 and Application Example 12, it can be seen that when the ketone-containing functional monomer is introduced into the pre-emulsion in step (S1), part of the ketone groups in the ketone-containing functional monomer are wrapped in the latex particles, resulting in a decrease in the ketone groups on the surface of the latex particles in the prepared ketone-containing polyacrylate emulsion, and a decrease in ketone hydrazine cross-linking, which deteriorates the wet and dry rubbing color fastness of the printing paste, and the printing changes color when washed with water, and the elasticity deteriorates.

[0225] From the comparison between Application Example 1 and Application Example 13, it can be seen that the soft monomer is reduced, the glass transition temperature is increased, the surface becomes dry, the wipe resistance of the printing paste is improved, and the dry and wet rubbing color fastness is improved, but the printing feel will become hard and crack after washing.

[0226] From the comparison between Application Example 4 and Comparative Application Example 1, it can be seen that when the amount of polyol in the preparation raw materials of the hydrazine-containing polyurethane emulsion is too small, the hard segment increases, the printing feel becomes harder, the elasticity becomes worse, the printing cracks after washing, and the color fastness to wet and dry rubbing becomes worse.

[0227] From the comparison between Application Example 4 and Comparative Application Example 2, it can be seen that when the amount of polyol used in the preparation raw materials of the hydrazine-containing polyurethane emulsion is too much, the printing feel will become soft, the printing color fastness will deteriorate, the dry and wet rubbing color fastness will deteriorate, and the color will fade when washed.

[0228] From the comparison between Application Example 1 and Comparative Application Example 3, it can be seen that when the hydrazine group in the polyurethane-polyacrylate composite emulsion is excessive, the polyurethane emulsion content increases, the hand feel becomes harder, the ketone group decreases, resulting in insufficient crosslinking, poor elasticity, poor water resistance, poor dry and wet rubbing color fastness, and fading when washed.

[0229] From the comparison between Application Example 1 and Comparative Application Example 4, it can be seen that when there are too few hydrazine groups in the polyurethane-polyacrylate composite emulsion, the polyacrylate emulsion content increases and the hand feels soft. The reduction of hydrazine groups leads to insufficient crosslinking, poor elasticity, poor water resistance, poor wet and dry rubbing, and discoloration after washing.

[0230] From the comparison between Application Example 1 and Comparative Application Example 5, it can be seen that when only the ketone-containing polyacrylate emulsion is used, due to the lack of cross-linking of the ketone group and the hydrazine group, the dry and wet rubbing color fastness deteriorates, the printing fades and peels, and the elasticity deteriorates.

[0231] The applicant declares that the present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A polyurethane-polyacrylate composite emulsion, characterized in that: The raw materials for preparing the polyurethane-polyacrylate composite emulsion include a combination of a hydrazine-containing polyurethane emulsion and a ketone-containing polyacrylate emulsion; The molar ratio of the hydrazine group in the hydrazine group-containing polyurethane emulsion to the ketone group in the ketone group-containing polyacrylate emulsion is (0.25-2):1; In parts by weight, the raw materials for preparing the hydrazine-containing polyurethane emulsion include 150-400 parts by weight of polyol, 60-180 parts by weight of polyisocyanate, 7-16 parts by weight of hydrophilic chain extender, 10-30 parts by weight of small molecule chain extender and 5-15 parts by weight of hydrazine-containing end-capping agent.

2. The polyurethane-polyacrylate composite emulsion according to claim 1, characterized in that: The number average molecular weight of the polyol is 600-3000; Preferably, the polyol includes any one or a combination of at least two of polycaprolactone diol, polycarbonate diol, polypropylene glycol, polytetrahydrofuran diol, polybutylene adipate, or castor oil; Preferably, the polyisocyanate includes any one or a combination of at least two of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate or hexamethylene diisocyanate; Preferably, the hydrophilic chain extender comprises a carboxylic acid type hydrophilic chain extender; Preferably, the carboxylic acid type hydrophilic chain extender comprises 2,2-dimethylol propionic acid and / or 2,2-dimethylol butyric acid; Preferably, the small molecule chain extender includes a polyamine chain extender; Preferably, the polyamine chain extender includes any one or a combination of at least two of isophoronediamine, ethylenediamine or diethylenetriamine; Preferably, the hydrazine-containing end-capping agent includes any one of adipic acid dihydrazide, oxalic acid dihydrazide, carbonate dihydrazide or succinic acid dihydrazide, or a combination of at least two thereof, and adipic acid dihydrazide and / or oxalic acid dihydrazide are further preferred; Preferably, the raw materials for preparing the hydrazine-containing polyurethane emulsion further include 7-16 parts by weight of a first neutralizer, 30-150 parts by weight of an organic solvent and 400-500 parts by weight of water; Preferably, the first neutralizing agent comprises triethylamine and / or triethanolamine; Preferably, the organic solvent comprises acetone and / or dimethylformamide; Preferably, the raw materials for preparing the hydrazine-containing polyurethane emulsion further include a catalyst; Preferably, the catalyst comprises an organobismuth catalyst; Preferably, based on 100% of the mass of the hydrazine-containing polyurethane emulsion, the mass of the catalyst is 0.1-1%.

3. The polyurethane-polyacrylate composite emulsion according to claim 2, characterized in that: The preparation method of the hydrazine-containing polyurethane emulsion comprises the following steps: (F1) reacting the polyol, the polyisocyanate and the hydrophilic chain extender to obtain a polyurethane prepolymer; (F2) mixing the polyurethane prepolymer with water for emulsification dispersion, adding the small molecule chain extender for a first reaction during and / or after the emulsification dispersion, and then adding the hydrazine-containing end-capping agent for a second reaction to obtain the hydrazine-containing polyurethane emulsion.

4. The polyurethane-polyacrylate composite emulsion according to claim 3, characterized in that: The reaction in step (F1) is carried out in the presence of the catalyst; Preferably, the reaction in step (F1) is carried out according to the following steps: (M1) pre-reacting the polyol with the polyisocyanate to obtain a first reaction system; (M2) the first reaction system reacts with the hydrophilic chain extender to obtain a second reaction system; (M3) the second reaction system reacts with the catalyst to obtain the polyurethane prepolymer; Preferably, the temperature of the pre-reaction is 80-120°C; Preferably, the pre-reaction time is 2-5h; Preferably, the reaction temperature in step (M2) is 40-80°C; Preferably, the reaction time in step (M2) is 1-3h; Preferably, the reaction temperature in step (M3) is 40-80°C; Preferably, the reaction time in step (M3) is 4-5h; Preferably, the emulsification dispersion temperature is 10-40°C; Preferably, the emulsification and dispersion time is 10-120 min; Preferably, the emulsification dispersion is carried out in the presence of the organic solvent; Preferably, before the mixing in step (F2), the step further includes the step of neutralizing the polyurethane prepolymer using the first neutralizing agent; Preferably, the neutralization temperature is 30-50°C; Preferably, the neutralization time is 10-15 min; Preferably, the temperature of the first reaction is 10-30°C; Preferably, the first reaction time is 20-60 min; Preferably, the temperature of the second reaction is 10-30°C; Preferably, the second reaction time is 30-60 min; Preferably, after the second reaction is completed, the method further comprises the step of removing the organic solvent.

5. The polyurethane-polyacrylate composite emulsion according to any one of claims 1 to 4, characterized in that: The raw materials for preparing the ketone-containing polyacrylate emulsion include polymerizable monomers; In parts by weight, the polymerizable monomers include 45-150 parts by weight of a hard monomer, 150-400 parts by weight of a soft monomer, and 5-10 parts by weight of a ketone-containing functional monomer; Preferably, the hard monomer includes any one or a combination of at least two of methyl methacrylate, styrene or acrylonitrile; Preferably, the soft monomer includes any one of ethyl acrylate, n-butyl acrylate or isooctyl acrylate, or a combination of at least two thereof; Preferably, the ketone group-containing functional monomer comprises diacetone acrylamide and / or ethyl acetoacetate methacrylate; Preferably, the polymerizable monomer further comprises a first functional monomer; the first functional monomer comprises any one or a combination of at least two of hydroxyethyl acrylate, acrylic acid, itaconic acid or methacrylic acid; Preferably, the first functional monomer is 5-10 parts by weight; Preferably, the total mass percentage of the ketone-containing functional monomer and the first functional monomer in the polymerizable monomer is 2-8%; Preferably, the mass percentage of the hard monomer in the polymerizable monomer is 10-45%; Preferably, the mass percentage of the soft monomer in the polymerizable monomer is 50-84%; Preferably, the raw materials for preparing the ketone-containing polyacrylate emulsion further include, by weight, 200-400 parts by weight of water, 1-15 parts by weight of anionic emulsifier, 0.5-5.5 parts by weight of nonionic emulsifier, 1.5-3.5 parts by weight of initiator, 0.1-1.5 parts by weight of buffer and 1-10 parts by weight of second neutralizer; Preferably, the anionic emulsifier comprises sodium dodecyl sulfate and / or sodium dodecylbenzene sulfonate; Preferably, the nonionic emulsifier comprises fatty alcohol polyoxyethylene ether; Preferably, the initiator comprises ammonium persulfate; Preferably, the initiator is dissolved in water and used in the form of an initiator aqueous solution; Preferably, the mass percentage of the initiator in the initiator aqueous solution is 0.2-5%; Preferably, the buffer comprises any one or a combination of at least two of disodium hydrogen phosphate, sodium bicarbonate or potassium hydroxide; Preferably, the second neutralizing agent comprises aqueous ammonia.

6. The polyurethane-polyacrylate composite emulsion according to claim 5, characterized in that: The preparation method of the ketone-containing polyacrylate emulsion comprises the following steps: (S1) mixing the hard monomer, the soft monomer, optionally the first functional monomer, water, the anionic emulsifier and the nonionic emulsifier to obtain a pre-emulsion; the pre-emulsion is divided into a first pre-emulsion, a second pre-emulsion and a third pre-emulsion; (S2) mixing the first pre-emulsion with water and performing a third reaction to obtain a seed emulsion; (S3) After the seed emulsion and the second pre-emulsion undergo a fourth reaction, the fourth pre-emulsion is added to sequentially undergo a fifth reaction and heat preservation to obtain the ketone-containing polyacrylate emulsion; the fourth pre-emulsion is composed of the third pre-emulsion and the ketone-containing functional monomer.

7. The polyurethane-polyacrylate composite emulsion according to claim 6, characterized in that: Taking the mass of the pre-emulsion as 100%, the mass of the first pre-emulsion is 4-6%, and the mass of the second pre-emulsion is 76-87.9%; Preferably, the solid content of the pre-emulsion is 45-90%; Preferably, the temperature of the third reaction is 50-70°C; Preferably, the third reaction time is 0.1-1h; Preferably, the mixed material in step (S2) further includes the buffer; Preferably, the third reaction, the fourth reaction and the fifth reaction are all carried out in the presence of the initiator; Preferably, the mass ratio of the initiator used in the third reaction, the fourth reaction and the fifth reaction is 1:(2-4):(1-2); Preferably, the temperature of the fourth reaction is 70-85°C; Preferably, the fourth reaction time is 2-4h; Preferably, the second pre-emulsion and the initiator are added to the reaction system in a dropwise manner; Preferably, the temperature of the fifth reaction is 70-85°C; Preferably, the fifth reaction time is 0.5-2h; Preferably, the fourth pre-emulsion and the initiator are added to the reaction system in a dropwise manner; Preferably, the insulation temperature is 80-82°C; Preferably, the insulation time is 1-3h; Preferably, after the heat preservation is completed, the step of adding the second neutralizing agent is also included; Preferably, the raw materials for preparing the polyurethane-polyacrylate composite emulsion further include a first defoaming agent; Preferably, the first defoamer comprises a polysiloxane defoamer and / or a mineral oil defoamer; Preferably, the mass percentage of the first defoamer in the polyurethane-polyacrylate composite emulsion is 0.2-1%.

8. A method for preparing the polyurethane-polyacrylate composite emulsion according to any one of claims 1 to 7, characterized in that: The preparation method comprises: Mixing a hydrazine-containing polyurethane emulsion with a ketone-containing polyacrylate emulsion to obtain the polyurethane-polyacrylate composite emulsion; Preferably, the mixed material further comprises a first defoaming agent.

9. A printing paste, characterized in that: The printing paste comprises the following components in parts by weight: 50-100 parts by weight of the polyurethane-polyacrylate composite emulsion according to any one of claims 1 to 7, 5-15 parts by weight of a moisturizer, 0.5-1 parts by weight of a third neutralizer, 0.3-2 parts by weight of an emulsifier, 0.1-1 parts by weight of a second defoaming agent, 1-5 parts by weight of a softener, and 1-3 parts by weight of a thickener.

10. The printing paste according to claim 9, characterized in that: The humectant includes glycerin and / or propylene glycol; Preferably, the third neutralizing agent comprises any one of triethanolamine, diethanolamine or triethylamine, or a combination of at least two thereof; Preferably, the emulsifier comprises isomeric tridecanol polyoxyethylene ether and / or primary alcohol polyoxyethylene ether; Preferably, the second defoamer comprises a mineral oil defoamer and / or a silicone defoamer; Preferably, the softener comprises diethylene glycol and / or dipropylene glycol dibenzoate; Preferably, the thickener comprises an alkali swellable thickener and / or a polyurethane associative thickener.