Method for synthesizing solid epoxy resin by using molten bisphenol A and solid epoxy resin
Through direct mixing of molten bisphenol A and liquid epoxy resin and high-temperature chain extension reaction, the problems of cooling granulation energy consumption and dust explosion are solved, and the efficient synthesis and process simplification of medium and high molecular weight solid epoxy resin is achieved, and the product quality is improved and production safety.
Patent Information
- Application Number
- CN202411227517.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, bisphenol A cooling granulation consumes a lot of energy, waste of packaging materials, and the transportation of solid particles has the risk of dust explosion and the health hazards of operators. In addition, the one-step method can only synthesize medium and low molecular weight epoxy resins.
The medium-high molecular weight solid epoxy resin is synthesized by using molten bisphenol A directly mixed with liquid epoxy resin, and the chain extension reaction is used to perform the heat of molten bisphenol A at high temperature. The process is simplified through a two-step process to avoid the risks of cooling granulation and dust explosion .
It saves energy and labor costs, improves the stability of product quality, and realizes simplification of the process and a production process without three wastes.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin materials, and in particular to a method for synthesizing solid epoxy resin by utilizing molten bisphenol A and the solid epoxy resin. Background Art
[0002] Epoxy resin is a general term for a class of polymers containing more than two epoxy groups in the molecule. It is a condensation product of bisphenol A and epichlorohydrin. Due to the chemical activity of the epoxy group, it can be opened with a variety of compounds containing active hydrogen, cured and cross-linked to form a network structure. Epoxy resin has excellent physical, mechanical and electrical insulation properties, adhesion to various materials, and flexible use process. It is widely used in coatings, composite materials, electronic appliances, adhesives and other fields. Among them, low-viscosity liquid epoxy resin is mainly used in high-end fields such as wind turbine blades, water-based coatings, electrical castings, carbon fiber composites, aerospace, etc.
[0003] In current industrial production, the synthesis methods of solid epoxy resins can be roughly divided into two types: one-step method and two-step method. The one-step process is to carry out polycondensation reaction of bisphenol A and epichlorohydrin under the action of liquid alkali, which is used to produce solid epoxy resins with medium relative molecular weight. The two-step process is to heat and dissolve bisphenol A and low relative molecular weight liquid bisphenol A type epoxy resin, and then carry out addition reaction under high temperature or catalyst, continuously extend the chain, and finally form medium and high molecular weight solid epoxy resin. In the one-step synthesis, the reaction is carried out in water as an emulsion. When preparing high relative molecular weight resins, post-treatment is more difficult. The relative molecular weight distribution of the obtained resin is relatively wide and the organic chlorine content is high. It is not easy to obtain products with high epoxy value and high softening point in the one-step method. The two-step reaction is carried out in a homogeneous phase, and the obtained resin has a large relative molecular weight and a narrow distribution. It has the advantages of simple process, convenient operation, less equipment, short working hours, no three wastes, one-time reaction, and easy control and adjustment of product quality. Therefore, it is increasingly valued.
[0004] Chinese patent CN103923299B discloses a production process for solid resin, which reacts bisphenol A and excess epichlorohydrin under reduced pressure and azeotropic dehydration under the action of a catalyst to remove unreacted ECH; dissolves the intermediate product with a solvent, and then adds alkali to continue the reaction; the solvent phase is washed, neutralized, and desolventized to obtain a solid epoxy resin, and high-salt wastewater is produced as a by-product. This method is a one-step method for preparing solid epoxy resin, with a long process and complex process. Organic solvents such as epichlorohydrin and toluene are used in the reaction process, high-salt wastewater is produced as a by-product, and the quality of the obtained resin product is difficult to control. Chinese patent CN104558518A discloses a method for directly synthesizing a basic epoxy resin using high-temperature liquid bisphenol A. This method mixes 170°C high-temperature molten BPA with 15°C ECH, and then performs an etherification reaction under the action of a catalyst, and finally prepares a liquid epoxy resin through steps such as cyclization, desolventization, and refining. This method requires molten bisphenol A to enter ECH in a tangential direction at a speed of 6 to 10 m / s, which is easy to cool and crystallize to block the pipeline, making the operation difficult. In addition, this method is to react bisphenol A and ECH to prepare liquid epoxy resin, and cannot prepare medium and high molecular weight solid epoxy resin. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a method for synthesizing a solid epoxy resin by using molten bisphenol A. The method comprises mixing molten bisphenol A directly with a liquid epoxy resin, and utilizing the heat of the high-temperature molten bisphenol A to heat a reaction system to carry out a chain extension reaction to synthesize a medium- and high-molecular-weight solid epoxy resin. The method aims to solve the problems in the prior art that bisphenol A has high energy consumption in cooling and granulating, wastes packaging materials, has dust explosion and poses health hazards to operators by using bisphenol A solid particles (powder), is difficult to transport solids, and has inaccurate metering, resulting in unstable quality indicators of the produced epoxy resin, and can only synthesize medium- and low-molecular-weight epoxy resins by the one-step method.
[0006] To achieve the above object, the present invention is implemented by the following specific technical scheme: A method for synthesizing solid epoxy resin using molten bisphenol A, comprising the following steps:
[0007] A method for synthesizing a solid epoxy resin using molten bisphenol A comprises the following steps:
[0008] a) mixing bisphenol A in a high temperature molten state and liquid epoxy resin uniformly in a static mixer, and adding the mixture into a reaction kettle;
[0009] b) Adding a catalyst into a reaction kettle and mixing uniformly, the mixture is subjected to addition reaction in an airtight condition, and the product is filtered, sliced, and packaged to obtain a solid epoxy resin.
[0010] Preferably, in step a), the melting temperature of bisphenol A is 160-190°C, and the temperature of the mixture of bisphenol A and liquid epoxy resin in a molten state is 120-150°C.
[0011] Preferably, in step a), the mixing ratio of bisphenol A to liquid epoxy resin is 0.2-0.6:1.
[0012] Preferably, in step b), the amount of catalyst added is 0 to 0.1%.
[0013] Preferably, in step b), the catalyst is one or more of bases, quaternary ammonium salts, triphenylphosphine and its derivatives, and imidazoles.
[0014] Preferably, in step b), the air-isolating condition is achieved by using nitrogen protection in the reactor or evacuating the reactor to a negative pressure, wherein the negative pressure in the reactor is set to -10 to -100 kPa.
[0015] Preferably, the reaction temperature of the addition reaction is 150-200° C., and the reaction time of the addition reaction is 1-5 h.
[0016] The invention also discloses a medium-high molecular weight solid epoxy resin synthesized by a method for synthesizing solid epoxy resin by using molten bisphenol A.
[0017] Compared with the prior art, the present invention has the following technical advantages:
[0018] 1. The molten bisphenol A is directly mixed with the liquid epoxy resin without going through the steps of cooling, granulation, packaging and transportation, and the heat of the high-temperature molten bisphenol A is used to heat the reaction system for chain extension reaction to synthesize medium- and high-molecular-weight solid epoxy resin, saving energy, packaging and labor costs;
[0019] 2. Bisphenol A solid particles have the risk of dust explosion during transportation. By adopting the technical solution of the present invention, bisphenol A is transported in the pipeline in the form of molten liquid, without the risk of dust explosion, and does not require forklift loading and unloading, manual unpacking, thus avoiding the harm of bisphenol A dust to operators;
[0020] 3. The two-step method is used to synthesize solid epoxy resin, which has the advantages of simple process, convenient operation, no three wastes, and easy control of product quality. DETAILED DESCRIPTION
[0021] In order to better understand the present invention, the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.
[0022] The purpose of the present invention is to provide a method for synthesizing medium- and high-molecular-weight solid epoxy resins by using molten bisphenol A, aiming to solve the problems in the prior art that the cooling and granulation of bisphenol A consumes a lot of energy and wastes packaging materials; the use of bisphenol A solid particles (powder) has dust explosion and harms the health of operators; the solid transportation is difficult and the metering is inaccurate, resulting in unstable quality indicators of the produced epoxy resin; and the one-step method can only synthesize medium- and low-molecular-weight epoxy resins.
[0023] The technical solution of the present invention directly mixes molten bisphenol A with liquid epoxy resin without cooling, granulation, packaging and transportation, and utilizes the heat of high-temperature molten bisphenol A to heat the reaction system for chain extension reaction to synthesize medium- and high-molecular-weight solid epoxy resin, thereby saving energy, packaging and labor costs. Bisphenol A solid particles have the risk of dust explosion during transportation. By adopting the technical solution of the present invention, bisphenol A is transported in the form of molten liquid in a pipeline without the risk of dust explosion, and does not require forklift loading and unloading, manual unpacking, and avoids the harm of bisphenol A dust to operators. The two-step method for synthesizing solid epoxy resin has the advantages of simple process, convenient operation, no three wastes, and easy control of product quality.
[0024] The present invention discloses a method for synthesizing a solid epoxy resin by using molten bisphenol A, comprising the following steps:
[0025] a) mixing bisphenol A in a high temperature molten state and liquid epoxy resin uniformly in a static mixer, and adding the mixture into a reaction kettle;
[0026] b) Adding a catalyst into a reaction kettle and mixing uniformly, the mixture is subjected to addition reaction in an airtight condition, and the product is filtered, sliced, and packaged to obtain a solid epoxy resin.
[0027] In an embodiment of the present invention, in step a), the melting temperature of bisphenol A is 160-190°C, and the temperature of the mixture of bisphenol A and liquid epoxy resin in a molten state is 120-150°C.
[0028] In an embodiment of the present invention, in step a), the mixing ratio of bisphenol A to liquid epoxy resin is 0.2-0.6:1.
[0029] In an embodiment of the present invention, in step b), the amount of catalyst added is 0-0.1%, preferably 0.01-0.05%.
[0030] In an embodiment of the present invention, in step b), the catalyst is one or more of bases, quaternary ammonium salts, triphenylphosphine and its derivatives, and imidazoles.
[0031] Wherein, the alkali catalyst is a mixed solution of one or more of NaOH, KOH, and LiOH;
[0032] The quaternary ammonium salt catalyst includes one or more of benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltrimethylammonium bromide, and benzyltriethylammonium bromide;
[0033] Triphenylphosphine and its derivatives include one or more of methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide and their derivatives;
[0034] The imidazole catalyst includes one or more of 2-methylimidazole, 2-propylimidazole, 2-11 alkylimidazole, 2-17 alkylimidazole, 2-metronidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, and 1-benzyl 2-methylimidazole.
[0035] In an embodiment of the present invention, in step b), the air isolation condition is achieved by using nitrogen protection in the reactor or evacuating the reactor to a negative pressure, wherein the negative pressure in the reactor is set to -10 to -100 kPa, preferably -50 to -90 kPa.
[0036] In the embodiment of the present invention, the reaction temperature of the addition reaction is 150-200° C., and the reaction time of the addition reaction is 1-5 h, preferably 1.5-3.5 h.
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0038] Example 1
[0039] In this embodiment, the liquid epoxy resin is selected from Nan Ya NPEL127 bisphenol A liquid epoxy resin.
[0040] By flow control, 160°C molten bisphenol A and NPEL127 bisphenol A type liquid epoxy resin were mixed uniformly in a static mixer at a mass ratio of 0.28:1. The temperature after mixing was 122.1°C, and the mixture was added to the reactor;
[0041] 0.01% NaOH catalyst was added into the reactor and mixed evenly. The addition reaction was carried out for 1.5 hours at 150° C. under nitrogen protection. The product was filtered, sliced and packaged to obtain a solid epoxy resin product.
[0042] Example 2
[0043] In this embodiment, the liquid epoxy resin is selected from Nan Ya NPEL127E bisphenol A liquid epoxy resin.
[0044] By flow control, 165°C molten bisphenol A and Nan Ya NPEL127E bisphenol A type liquid epoxy resin were mixed uniformly in a static mixer at a mass ratio of 0.32:1. The temperature after mixing was 128.5°C, and the mixture was added into the reactor;
[0045] 0.015% of benzyltrimethylammonium chloride catalyst was added to the reactor and mixed evenly. After nitrogen replacement, the pressure in the reactor was set to -20 kPa and the temperature was set to 160°C. The addition reaction was carried out for 2.5 hours. The product was filtered, sliced and packaged to obtain a solid epoxy resin product.
[0046] Example 3
[0047] In this embodiment, the liquid epoxy resin is selected from Nan Ya NPEL127E bisphenol A liquid epoxy resin.
[0048] By flow control, 170°C molten bisphenol A and Nan Ya NPEL127E bisphenol A type liquid epoxy resin were mixed uniformly in a static mixer at a mass ratio of 0.37:1. The temperature after mixing was 131.3°C, and the mixture was added into the reactor;
[0049] 0.02% benzyltriethylammonium chloride and 2-methylimidazole catalyst were added into the reactor and mixed evenly (mixing ratio 1:1). After nitrogen replacement, the pressure in the reactor was set to -40 kPa and the temperature was set to 170°C. The addition reaction was carried out for 3 hours. The product was filtered, sliced and packaged to obtain a solid epoxy resin product.
[0050] Example 4
[0051] In this embodiment, the liquid epoxy resin is selected from Nan Ya NPEL128 bisphenol A liquid epoxy resin.
[0052] By flow control, 175°C molten bisphenol A and Nan Ya NPEL128 bisphenol A type liquid epoxy resin were mixed uniformly in a static mixer at a mass ratio of 0.39:1. The temperature after mixing was 136.7°C, and the mixture was added to the reactor;
[0053] 0.025% ethyltriphenylphosphonium bromide and KOH catalyst were added into the reactor and mixed evenly (mixing ratio 5:1). After nitrogen substitution, the pressure in the reactor was set to -60 kPa and the temperature was set to 180°C. The addition reaction was carried out for 2 hours. The product was filtered, sliced and packaged to obtain a solid epoxy resin product.
[0054] Example 5
[0055] In this embodiment, the liquid epoxy resin is selected from Nan Ya NPEL128 bisphenol A liquid epoxy resin.
[0056] By flow control, 180°C molten bisphenol A and Nan Ya NPEL128 bisphenol A type liquid epoxy resin were mixed uniformly in a static mixer at a mass ratio of 0.47:1. The temperature after mixing was 141.6°C, and the mixture was added into the reactor;
[0057] 0.03% propyltriphenylphosphonium bromide and 2-ethyl-4-methylimidazole catalyst were added to the reactor and mixed evenly (mixing ratio 2:1). After nitrogen replacement, the pressure in the reactor was set to -70 kPa and the temperature was set to 190°C. The addition reaction was carried out for 3 hours. The product was filtered, sliced and packaged to obtain a solid epoxy resin product.
[0058] Example 6
[0059] In this embodiment, the liquid epoxy resin is selected from Nan Ya NPEL128E bisphenol A liquid epoxy resin.
[0060] By flow control, 190°C molten bisphenol A and Nan Ya NPEL128E bisphenol A type liquid epoxy resin were mixed uniformly in a static mixer at a mass ratio of 0.52:1. The temperature after mixing was 146.5°C, and the mixture was added into the reactor;
[0061] 0.05% butyltriphenylphosphine bromide catalyst was added to the reactor and mixed evenly. After nitrogen substitution, the reactor pressure was set to -90 kPa and the temperature was set to 200°C. The addition reaction was carried out for 3.5 hours. The product was filtered, sliced and packaged to obtain a solid epoxy resin product.
[0062] The performance comparison of Examples 1 to 6 with Comparative Examples 1 and 2 of commercially available products is shown in the following table:
[0063]
[0064] Compared with the prior art, the method for synthesizing medium- and high-molecular-weight solid epoxy resin using molten bisphenol A disclosed in the present invention has the following beneficial effects: the molten bisphenol A is directly mixed with the liquid epoxy resin without going through the steps of cooling, granulation, packaging and transportation, and the heat of the high-temperature molten bisphenol A is used to heat the reaction system to carry out chain extension reaction to synthesize the medium- and high-molecular-weight solid epoxy resin, thereby saving energy, packaging and labor costs;
[0065] Bisphenol A solid particles have a risk of dust explosion during transportation. By adopting the technical solution of the present invention, bisphenol A is transported in the pipeline in the form of molten liquid, without the risk of dust explosion, and does not require forklift loading and unloading, manual unpacking, and avoids the harm of bisphenol A dust to operators;
[0066] The two-step method for synthesizing solid epoxy resin has the advantages of simple process, convenient operation, no three wastes, and easy control of product quality.
[0067] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A method for synthesizing solid epoxy resin using molten bisphenol A, It is characterized in that The following steps are involved: a) mixing bisphenol A in a high temperature molten state and liquid epoxy resin uniformly in a static mixer, and adding the mixture into a reaction kettle; b) Adding a catalyst into a reaction kettle and mixing uniformly, the mixture is subjected to addition reaction in an airtight condition, and the product is filtered, sliced, and packaged to obtain a solid epoxy resin.
2. The method for synthesizing solid epoxy resin using molten bisphenol A according to claim 1, It is characterized in that In the step a), the melting temperature of the bisphenol A is 160-190°C, and the temperature of the mixture of the bisphenol A and the liquid epoxy resin in a molten state is 120-150°C.
3. The method for synthesizing solid epoxy resin using molten bisphenol A according to claim 1, It is characterized in that In the step a), the mixing ratio of bisphenol A to liquid epoxy resin is 0.2-0.6:
1.
4. The method for synthesizing solid epoxy resin using molten bisphenol A according to claim 1, It is characterized in that In the step b), the amount of the catalyst added is 0 to 0.1%.
5. The method for synthesizing solid epoxy resin using molten bisphenol A according to claim 1, It is characterized in that In the step b), the catalyst is one or more of bases, quaternary ammonium salts, triphenylphosphine and its derivatives, and imidazoles.
6. The preparation method according to claim 1, characterized in that, in the step b), the air-isolating condition is achieved by using nitrogen protection in the reactor or evacuating the reactor to negative pressure. in, The negative pressure in the reactor was set to -10 to -100 kPa.
7. The method according to claim 1, It is characterized in that The reaction temperature of the addition reaction is 150-200° C., and the reaction time of the addition reaction is 1-5 hours.
8. A medium-high molecular weight solid epoxy resin synthesized by the method for synthesizing a solid epoxy resin using molten bisphenol A as claimed in any one of claims 1 to 7.