Multi-component copolyester and preparation method thereof

By using initial depolymerization, repolymerization, esterification and polycondensation steps in the preparation process of regenerated PBAT, and using low-content catalysts and chelating agents, a multi-copolyester with low heavy metal content was prepared, which solved the high heavy metals in the prior art , The problem of poor printing performance improves biodegradability and tensile strength, and is suitable for packaging and agricultural films.

CN118930823AActive Publication Date: 2024-11-12NAT POLYMER MATERIALS IND INNOVATION CENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310526959.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The existing recycled PBAT has high heavy metal content and poor printing performance, which limits its application range and lacks biodegradation and tensile strength.

Method used

By adopting a preparation method of multi-polymerized copolyester, through the initial depolymerization, re-depolymerization, esterification and polycondensation steps, a low content of depolymerization catalyst and chelating agent are used to prepare multi-polymerized copolyester with extremely low heavy metal content. It includes 35 to 65 mol% of aliphatic and aromatic dicarboxylic acid, 1,4-butanediol and a small amount of third monomer, with a crystallinity of 5 to 22%, and is made of waste polyester as raw material.

Benefits of technology

It has achieved a reduction in the heavy metal content in multi-copolyesters, improved printing performance and biodegradation performance, enhanced tensile strength, and is suitable for disposable packaging films and agricultural film fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930823A_ABST
    Figure CN118930823A_ABST
Patent Text Reader

Abstract

The invention provides multi-component copolyester and a preparation method thereof, and belongs to the technical field of polyester. The multi-component copolyester comprises a component A and a dicarboxylic acid compound, and based on the total molar weight of the component A, the multi-component copolyester comprises: a1, 35-65 mol% of aliphatic dicarboxylic acid; a2, 35-65 mol% of aromatic dicarboxylic acid or a derivative thereof; the component B is 1, 4-butanediol; based on the total molar weight of the component B and the component C, the component C accounts for 5-30 mol%; the crystallinity of the multi-component copolyester is 5-22%, the zinc content in the multi-component copolyester is less than or equal to 100 ppm, and the titanium content in the multi-component copolyester is less than or equal to 120 ppm. According to the multi-component copolyester disclosed by the invention, the waste polyester is taken as a raw material, and the multi-component copolyester with low heavy metal content, proper crystallinity, good printing performance and good biodegradability is prepared through the steps of primary alcoholysis, secondary alcoholysis, ester exchange and polycondensation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of recycled polyester, in particular to a multi-component copolyester and a preparation method thereof. Background Art

[0002] At present, globally, degradable plastics account for about 58% of plastic production, and non-degradable plastics account for 42%. The treatment of waste plastics is an urgent problem to be solved. In the future, my country will gradually solve the harm caused by traditional waste plastic treatment to the environment through source reduction, reuse, use of bio-based or biodegradable plastics instead of fossil-based materials, and plastic recycling through physical or chemical recycling. Among them, the primary products of chemical recycling are mainly monomers and oligomers such as DMT, TPA, EG, BHET, and BHETA, and the secondary products are mainly synthetic PET, UPR, ERD, VER, AR, PU, ​​UPP, NPS, PIF, OP, AD, PBAT, etc.

[0003] Polybutylene terephthalate adipate (PBAT) is a fully biodegradable polyester. Due to its good toughness, film-forming properties and easy blowing, it has been widely used in the field of disposable packaging films and agricultural films. In the prior art, there have been some reports on the preparation of regenerated PBAT. For example, Chinese patent application CN112724388A discloses a production device for recycling polyester to regenerate a degradable material PBAT. The dried recycled PET is alcoholyzed in an alcoholysis reaction system to obtain crude BHET, and then the BHET monomer is obtained through a dealcoholization system. It is reacted with BDO in the first esterification reaction system to obtain BHBT monomer, and the AA ester is reacted in the second esterification reaction system to obtain a copolyester, and then the weight-average molecular weight is increased by polycondensation through a pre-polycondensation reaction system and a final polycondensation reaction system to obtain a PBAT product. However, the strength of PBAT is poor, especially the tensile strength is low. PBAT usually needs to be added with calcium powder or blended with PLA to have better physical properties. PBAT has problems such as mechanical properties that cannot meet the use requirements during use, which limits the application range of PBAT.

[0004] There are prior art reports that PBAT is modified to obtain a multi-component copolyester to improve the mechanical properties of the material. For example, CN 112080000 A discloses a method for synthesizing poly(terephthalic acid-adipic acid-meta-epoxypentadecylphenol) butanediol (PBATE material), which is synthesized from PBAT and meta-epoxypentadecylphenol, and the mechanical properties of the material are better than those of PBAT; CN 113861399 A discloses a biodegradable polyester poly(isosorbide terephthalic acid-butylene adipate) (PBIAT) and a preparation method thereof, the preparation method comprising uniformly mixing 27-23% adipic acid, 31-26% terephthalic acid, 6-48% isosorbide and 36-3% butanediol, adding the mixture to a reactor to react, then adding a catalyst to raise the temperature for polycondensation to obtain PBIAT polyester. However, the multi-component copolyesters reported in the prior art are not made from waste polyester as raw materials.

[0005] In addition, for recycled PBAT copolyesters, the existing technology (Zhang Hongming, Zhao Junyu, Gao Fengxiang, et al. Study on the depolymerization-cocondensation "one-pot" synthesis of biodegradable polymers of PET [J]. Journal of Polymer Science, 2022(009):053.) uses diols of different structures to hydrolyze PET into low molecular weight prepolymers, and then adds dibasic acids for further esterification and polycondensation, so that the depolymerization and copolymerization of PET are completed by the "one-pot method". However, since the recycled materials usually contain different amounts of heavy metals, and heavy metal catalysts are also used in the depolymerization process, the catalyst residue will seriously affect the physical properties and aging resistance of the product. The current petroleum-based biodegradable plastic PBAT has high production costs and relatively slow biodegradability. In addition, since PBAT is mainly used for packaging bags, the packaging bags generally need to be printed with patterns, patterns or texts. If the printing performance is poor, the ink printing will easily fade, thereby affecting the appearance and safety of the packaging bags.

[0006] Therefore, it is necessary to provide a multi-component copolyester, which has low residual heavy metal content, better degradation performance, better toughness and tensile strength, low carbon emission value, and better printing performance. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects of high heavy metal content and poor printing performance in the prior art and to provide a multi-component copolyester.

[0008] Another object of the present invention is to provide a method for preparing the above-mentioned multi-component copolyester.

[0009] To achieve the above object, the present invention adopts the following technical solution:

[0010] A multi-component copolyester, comprising:

[0011] Component A, a dicarboxylic acid compound, based on the total molar amount of component A, comprises:

[0012] a1, 35 to 65 mol% of at least one aliphatic dicarboxylic acid;

[0013] a2, 35 to 65 mol% of at least one aromatic dicarboxylic acid or a derivative thereof;

[0014] Component B, 1,4-butanediol;

[0015] Component C, a third monomer, based on the total molar amount of component B and component C, the component C accounts for 5 to 30 mol%; the third monomer is at least one of ethylene glycol, 1,4-cyclohexanedimethanol, and isosorbide;

[0016] The crystallinity of the multi-component copolyester is 5-22%, including but not limited to 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, and 22%; the zinc content in the multi-component copolyester is ≤100ppm, and the titanium content is ≤120ppm.

[0017] The monomers of the multi-component copolyester of the present invention include aliphatic-aromatic dicarboxylic acid compounds, 1,4-butanediol and a small amount of a third monomer, and have extremely low metal ion content, wherein the zinc content is ≤100ppm, the titanium content is ≤120ppm, and the crystallinity is 5-22%. The multi-component copolyester has good degradability, good tensile properties and good printing properties.

[0018] The zinc and titanium residues in the multi-component copolyester of the present invention are introduced by the catalyst used in the depolymerization and polycondensation processes on the one hand, and by the impurities in the waste polyester raw materials on the other hand.

[0019] Preferably, the zinc content in the multi-component copolyester is 45-70 ppm, and the titanium content is 50-105 ppm.

[0020] Preferably, the calcium content in the multi-component copolyester is ≤71 ppm.

[0021] More preferably, the calcium content in the multi-component copolyester is 35 to 60 ppm.

[0022] Preferably, the silicon content in the multi-component copolyester is ≤85ppm.

[0023] More preferably, the silicon content in the multi-component copolyester is 35 to 50 ppm.

[0024] The residual calcium and silicon in the multi-polymer copolyesters are mainly due to the introduction of impurities in the polyester raw materials.

[0025] In the present invention, the crystallinity of the multi-copolyester is analyzed using an X-ray diffractometer (XRD) with reference to standard JY / T0587-2020. Specifically, a D8 ADVANCE X-ray diffractometer from BRUKER, Germany, is used, at room temperature, CuKa rays (λ=0.154 nm), collected once every 0.05°, and the scanning angle range is 6° to 60°.

[0026] In the present invention, the zinc content and the titanium content are tested according to the following method:

[0027] Inductively coupled plasma atomic emission spectrometer ICP-OES was used according to the standard inductively coupled plasma atomic emission spectrometer determination method US EPA 6010C:2014.

[0028] Preferably, the melting point of the multi-copolyester is 105-140°C, including but not limited to 105°C, 107°C, 109°C, 111°C, 113°C, 115°C, 117°C, 119°C, 121°C, 123°C, 125°C, 127°C, 129°C, 131°C, 133°C, 135°C, 137°C, 139°C, and 140°C.

[0029] The melting point of the multi-copolyester was tested using a differential scanning calorimeter in accordance with standard ISO 11357-3:2018.

[0030] Preferably, the relative viscosity of the multi-copolyester is 1.2 to 1.8, including but not limited to 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, and 1.8.

[0031] The relative viscosity of the multi-copolyester is tested as follows:

[0032] According to the GB / T 17931-1999 standard method, the sample concentration was 5 mg / ml in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05°C.

[0033] Preferably, the terminal carboxyl content of the multi-copolyester is 13 to 30 mmol / t, including but not limited to 13 mmol / t, 14 mmol / t, 15 mmol / t, 16 mmol / t, 17 mmol / t, 18 mmol / t, 19 mmol / t, 20 mmol / t, 21 mmol / t, 22 mmol / t, 23 mmol / t, 24 mmol / t, 25 mmol / t, 26 mmol / t, 27 mmol / t, 28 mmol / t, 29 mmol / t, and 30 mmol / t.

[0034] The terminal carboxyl content is tested as follows:

[0035] The terminal carboxyl content is tested according to standard FZ / T 50012-2006 using automatic potentiometric titration analysis.

[0036] Preferably, the weight average molecular weight of the multi-component copolyester is 40,000-100,000, including but not limited to 40,000, 45,000, 50,000, 55,000, 60,000, 65,000, 70,000, 75,000, 80,000, 85,000, 90,000, 95,000, and 100,000.

[0037] The weight average molecular weight is tested as follows:

[0038] According to the standard GB / T 21863-2008 gel permeation chromatography (GPC), an ultra-high performance polymer chromatograph (APC) was used, tetrahydrofuran was used as the eluent, a differential detector was used as the detector, the column temperature was 40°C, and the flow rate was 0.5 mL / min.

[0039] Preferably, the aliphatic dicarboxylic acid is selected from at least one of malonic acid, succinic acid, adipic acid, sebacic acid, pimelic acid, suberic acid, and azelaic acid, and the aromatic dicarboxylic acid or its derivative is selected from at least one of terephthalic acid or its derivative, and isophthalic acid or its derivative.

[0040] The present invention also protects a method for preparing the above-mentioned multi-component copolyester, comprising the following steps:

[0041] S1. Initial depolymerization:

[0042] Dissolving waste terephthalic acid polyester in an alcohol solvent containing a depolymerization catalyst, and carrying out a primary depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions to obtain a primary depolymerization product;

[0043] The temperature of the initial depolymerization reaction is 180-230°C and the time is 15-120 minutes;

[0044] S2. Re-depolymerization:

[0045] Extracting part of the diol from the primary depolymerization product obtained in step S1, adding a chelating agent, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions, and filtering the reactant to obtain a filtrate as the re-depolymerization product;

[0046] The temperature of the re-depolymerization reaction is 160-190°C and the time is 10-20 minutes;

[0047] S3. Esterification reaction:

[0048] According to the monomer content of the multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield reaches 90%, to obtain an esterified product;

[0049] S4. Polycondensation:

[0050] After removing excess alcohol solvent from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum conditions to obtain the multi-component copolyester.

[0051] The preparation method of the multi-component copolyester of the invention uses waste polyester as raw material and prepares the multi-component copolyester with low heavy metal content and suitable crystallinity through the steps of two alcoholysis, esterification reaction and polycondensation.

[0052] In the initial depolymerization step, the waste polyester is preliminarily depolymerized in the presence of a depolymerization catalyst under normal pressure, inert gas atmosphere, and microwave conditions. The temperature of the initial depolymerization reaction is relatively high, and most of the waste polyester is depolymerized into monomers or oligomers. Then, part of the ethylene glycol is extracted from the product of the initial depolymerization, and after adding a chelating agent, a second depolymerization, i.e., re-depolymerization, is performed. The temperature of the re-depolymerization is lower than that of the initial depolymerization, and the time is shorter. Under the action of the chelating agent, most of the heavy metal ions in the waste polyester are removed synchronously during the re-depolymerization process, and the addition of the chelating agent will not have a negative impact on the printing performance or crystallinity of the polyester.

[0053] In the preparation method of the present invention, part of the diol is extracted in step S2, and the diol is a depolymerization byproduct, and an aliphatic dicarboxylic acid and a third monomer are added in step S3, all in order to obtain a multi-component copolyester with an appropriate monomer content. The monomer content of the finally obtained multi-component copolyester meets the following range: component A, a dicarboxylic acid compound, based on the total molar amount of component A, includes: a1, 35 to 65 mol% of at least one aliphatic dicarboxylic acid; a2, 35 to 65 mol% of at least one aromatic dicarboxylic acid or its derivative; component B, 1,4-butanediol; component C, a third monomer, based on the total molar amount of component B and component C, the component C accounts for 5 to 30 mol%.

[0054] The method for extracting part of the ethylene glycol in step S2 may be reduced pressure distillation.

[0055] Preferably, the waste polyester includes one or more of recycled polyethylene terephthalate (PET), polybutylene terephthalate (PBT), PET / PBT alloy, and PBAT.

[0056] Optionally, sources of the waste polyester include but are not limited to post-consumer recycled plastics (Post Consumer Recycled Plastic, PCR), industrial recycled plastics (Post Industry Recycle Plastic, PIR), ocean bound plastics (Ocean Bound Plastic, OBP), and in the ocean plastics (IOP).

[0057] Preferably, the waste polyester further includes the steps of impurity removal, cleaning and crushing before the initial depolymerization.

[0058] Preferably, in step S2, the chelating agent is a biomass chelating agent.

[0059] Preferably, the chelating agent includes at least one of stearyl citrate, calcium citrate, tea polyphenols and phytic acid.

[0060] More preferably, the chelating agent is tea polyphenols.

[0061] Tea polyphenols as chelating agents can not only efficiently complex residual metal ions in waste polyester, but also help stabilize the reaction system and reduce yellowing of products for multi-copolyesters.

[0062] Preferably, in step S2, the amount of the chelating agent added is 0.01-0.1 wt.% of the waste polyester.

[0063] The chelating agent can be added in a relatively low amount to effectively remove metal ions from waste polyester.

[0064] Preferably, in step S1, the depolymerization catalyst includes at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate.

[0065] Preferably, in step S1, the amount of the depolymerization catalyst added is 0.05-0.5 wt.% of the waste polyester.

[0066] Preferably, the alcohol solvent includes at least one of 1.4-butanediol and ethylene glycol.

[0067] Preferably, the mass ratio of the waste polyester to the alcohol solvent is 1:0.8 to 1:2.

[0068] Preferably, the polymerization catalyst and the polycondensation catalyst are each independently selected from at least one of butyl titanate, tetraisopropyl titanate, titanium phosphorus compounds, titanium silicon compounds, titanium magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide.

[0069] Preferably, in step S3, the aliphatic dicarboxylic acid is adipic acid and / or sebacic acid.

[0070] Since the waste polyester is depolymerized in step S1 and step S2, some aliphatic alcohol already exists in the depolymerization product, and a certain amount of aliphatic alcohol is added in step S3 to make the alcohol in the whole reaction system excessive.

[0071] The stabilizer is one or more of organic phosphites, trimethyl phosphates, and hindered phenols.

[0072] Optionally, the organic phosphite stabilizer may be one or more of trimethyl phosphite, triethyl phosphite or triphenyl phosphite.

[0073] Optionally, the phosphate stabilizer may be one or more of triphenyl phosphate, trimethyl phosphate or triethyl phosphate.

[0074] Optionally, the hindered phenol stabilizer may be 3,5-di-tert-butyl-4-hydroxybenzyl diethylphosphonate (antioxidant 1222) and / or antioxidant 1010.

[0075] The chain extender is at least one of pentaerythritol, trimethylolethane, trimethylolpropane (TMP), xylitol, sorbitol, HDI, MDI, TDI, isophorone diisocyanate, ethylene-methyl methacrylate copolymer (EMA), and multifunctional epoxy compound ADR.

[0076] Preferably, the added amount of the chain extender is 0 to 0.1 wt.% of the waste polyester.

[0077] Preferably, in step S3, the temperature of the esterification reaction is 170-210° C., and the time is 1-2 h.

[0078] Preferably, in step S3, the amount of the polymerization catalyst added is 0.01-0.1 wt.% of the waste polyester.

[0079] Preferably, in step S4, the amount of the polycondensation catalyst added is 0.03-0.1 wt.% of the waste polyester.

[0080] Preferably, in step S4, the temperature of the polycondensation reaction is 240-250° C., the time is 2-5 hours, and the pressure is 20-100 Pa.

[0081] Preferably, in step S1, the microwave reaction conditions are as follows: frequency 2450 Hz, temperature 180-230° C., and time 15-120 min.

[0082] Preferably, in step S2, the microwave reaction conditions are as follows: frequency 2450 Hz, temperature 160-190° C., and time 10-20 min.

[0083] Compared with the prior art, the present invention has the following beneficial effects:

[0084] The present invention develops a multi-component copolyester and a preparation method thereof. The multi-component copolyester of the present invention uses waste polyester as raw material, and is prepared through the steps of primary alcoholysis, secondary alcoholysis, esterification reaction and polycondensation to obtain a multi-component copolyester with low heavy metal content and suitable crystallinity.

[0085] The initial depolymerization and the re-depolymerization are carried out under microwave conditions, wherein the re-depolymerization includes the addition of a chelating agent, and the addition of the chelating agent and the reaction of the re-depolymerization act synergistically to remove most of the metal ion residues in the waste polyester, and the obtained multi-component copolyester has an extremely low heavy metal content, wherein the zinc content is ≤100ppm and the titanium content is ≤120ppm.

[0086] Since the multi-component copolyester of the present invention has extremely low heavy metal content and a good crystallinity range, the obtained multi-component copolyester has excellent printing performance and good biodegradability, and can be widely used in the field of disposable packaging films and agricultural films. BRIEF DESCRIPTION OF THE DRAWINGS

[0087] Figure 1 is the infrared spectrum of the multi-component copolyester of Example 1;

[0088] Figure 2 is the H NMR spectrum of the multi-component copolyester of Example 1;

[0089] Figure 3 is the XRD pattern of the multi-component copolyester of Example 1;

[0090] Figure 4 This is the GPC chart of the multi-component copolyester of Example 1. DETAILED DESCRIPTION

[0091] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form.

[0092] The raw materials in the embodiments and comparative examples of the present invention can be obtained from commercial sources;

[0093] in:

[0094] Waste polyester-1, PET, recycled from electronic pallet materials;

[0095] Waste polyester-2, rPET-pellet, recycled from Indonesian ocean plastic;

[0096] Waste polyester-3, PET / PBT, recycled PET / PBT alloy;

[0097] Waste polyester-4, PBAT, recycled PBAT waste;

[0098] Condensation catalyst and polymerization catalyst: butyl titanate, purchased from Aladdin;

[0099] Depolymerization catalyst: zinc acetate, purchased from Aladdin;

[0100] Chain extender: trimethylolpropane;

[0101] Chelating agents: tea polyphenols, stearyl citrate, and phytic acid, all purchased from Maclean;

[0102] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.

[0103] Embodiments 1 to 4

[0104] Examples 1 to 4 provide a method for preparing a multi-component copolyester, respectively, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 1:

[0105] S1. Initial depolymerization:

[0106] Waste polyester with an average particle size of ≤2 mm is dissolved in an alcohol solvent containing a depolymerization catalyst, placed in a microwave reactor (Yantai Haoming Microwave Company), and subjected to a primary depolymerization reaction under a nitrogen atmosphere and microwave conditions to obtain a primary depolymerization product; the microwave conditions are: a frequency of 2450 Hz.

[0107] S2. Re-depolymerization:

[0108] By vacuum distillation, part of the diol is extracted from the primary depolymerization product obtained in step S1, and a chelating agent is added, and the product is placed in a microwave reactor to carry out a re-depolymerization reaction under normal pressure, an inert gas atmosphere and microwave conditions. After the reactants are filtered, the filtrate obtained is the re-depolymerization product; the microwave conditions are: a frequency of 2450HZ.

[0109] S3. Esterification reaction:

[0110] According to the monomer content of the target multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield reaches 90%, to obtain an esterified product;

[0111] S4. Polycondensation:

[0112] After removing excess alcohol from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum conditions to obtain the multi-component copolyester.

[0113] Table 1 Raw materials and reaction conditions of Examples 1 to 4

[0114]

[0115]

[0116] Embodiments 5 to 10

[0117] Embodiments 5 to 10 provide a method for preparing a multi-component copolyester. Except for step S2, the other steps are the same as those of embodiment 1. Specifically, the preparation methods of embodiments 5 to 10 differ from those of embodiment 1 in that:

[0118] In Example 5, the type of chelating agent is tea polyphenols;

[0119] The type of chelating agent in Example 6 is stearyl citrate;

[0120] In Example 7, the proportion of the chelating agent to the waste polyester is 0.01 wt.%;

[0121] In Example 8, the proportion of the chelating agent to the waste polyester is 0.1 wt.%;

[0122] The conditions for the re-depolymerization reaction in Example 9 were 190° C., 10 min;

[0123] The conditions for the re-depolymerization reaction in Example 10 are 160° C., 20 min.

[0124] The monomer ratios prepared in Examples 5-10 are shown in Table 2

[0125] Table 2 Monomer ratios in the multi-component copolyesters prepared in Examples 5-10

[0126]

[0127]

[0128] Comparative Examples 1 to 5

[0129] Comparative Examples 1 to 5 provide a method for preparing a multi-component copolyester, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 3:

[0130] S1. Initial depolymerization:

[0131] Dissolve the waste polyester with an average particle size of ≤2 mm in an alcohol solvent containing a depolymerization catalyst, place it in a microwave reactor (Yantai Haoming Microwave Company), and perform a primary depolymerization reaction under a nitrogen atmosphere and microwave conditions to obtain a primary depolymerization product;

[0132] S2. Re-depolymerization:

[0133] Extracting part of ethylene glycol from the primary depolymerization product obtained in step S1 by vacuum distillation, adding a chelating agent (or not adding a chelating agent), placing the product in a microwave reactor, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions. After filtering the reactant, the filtrate obtained is the re-depolymerization product;

[0134] S3. Esterification reaction:

[0135] According to the monomer content of the target multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield reaches 90%, to obtain an esterified product;

[0136] S4. Polycondensation:

[0137] After removing excess alcohol from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum conditions to obtain the multi-component copolyester.

[0138] Table 3 Raw materials and reaction conditions of Comparative Examples 1 to 5

[0139]

[0140]

[0141]

[0142] Performance Testing

[0143] The performance of the multi-component copolyesters prepared in the above examples and comparative examples was tested, and the specific method is as follows:

[0144] Melting point: ISO 11357-3:2018;

[0145] Relative viscosity: According to the GB / T 17931-1999 standard method, it is measured in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05℃, and the sample concentration is 5mg / ml;

[0146] Terminal carboxyl content: FZ / T 50012-2006;

[0147] Metal ion residue: US EPA 6010C:2014;

[0148] Crystallinity: JY / T 0587-2020;

[0149] Weight average molecular weight: detected by gel permeation chromatography (GPC);

[0150] 50-day biodegradation rate: According to GB / T 19277-2003 "Determination of the ultimate aerobic biodegradability and disintegration of materials under controlled composting conditions using the method of measuring the released carbon dioxide", the biodegradation performance is determined by the composting method.

[0151] Printing retention rate: in accordance with GB / T 38082-2019, Section 5.3.4 Printing quality test for biodegradable plastic shopping bags.

[0152] The multi-component copolyester prepared in Example 1 was subjected to infrared spectroscopy, nuclear magnetic hydrogen spectroscopy, and XRD, and the specific methods were:

[0153] Infrared spectrum: The sample preparation method adopts hot pressing film forming, the wave number range is 4000~400cm-1, the number of scans is 16 times, the resolution is 4, and the sampling method is transmission;

[0154] H-NMR spectrum: Deuterated trifluoroacetic acid was used as solvent and tetramethylsilane (TMS) was used as internal standard to test H-NMR spectrum;

[0155] XRD: X-ray diffractometer (XRD) was used according to standard JY / T 0587-2020.

[0156] Using XRD testing, the crystallization peak (sharp peak) and non-crystallization peak area (diffuse peak) are obtained, and the crystallinity is calculated according to the following formula:

[0157]

[0158] Where:

[0159] Wc-crystallinity

[0160] I C -Integrated area of ​​diffraction peak in crystalline state

[0161] I a -Integrated area of ​​diffraction peak of amorphous state

[0162] The infrared spectrum of the multi-component copolyester of Example 1 is shown in Figure 1 , NMR hydrogen spectrum see Figure 2 , XRD pattern see Figure 3 , GPC spectrum see Figure 4 .

[0163] The test results of the embodiments are shown in Table 4, and the test results of the comparative examples are shown in Table 4.

[0164] Table 4

[0165]

[0166]

[0167] Table 6

[0168]

[0169] According to the test results in Table 4, the crystallinity range of the multi-component copolyester obtained by the technical solution of the present invention is suitable, between 10-19.5%, and the heavy metal ion content is extremely low. The obtained product has excellent performance, among which the 50-day biodegradation rate is above 35%, and the printing peeling rate is below 7%. In addition, it can be seen from the infrared spectrum, nuclear magnetic hydrogen spectrum and other spectra of the multi-component copolyester obtained in Example 1 that the present invention successfully prepared PBATE and can calculate the proportion of different segments. Infrared spectrum analysis: Figure 1 1731cm shown -1 The carbonyl (-C=O) stretching vibration peak at 1104 cm -1 、1271cm -1 731cm is the stretching vibration peak of ether bond (COC). -1 It is the out-of-plane bending vibration peak of CH on the para-disubstituted benzene ring. The stretching vibration and out-of-plane bending vibration absorption peak of the (-CH) group at 3053cm-1 is attributed to the (-CH) group on the benzene ring. Figure 1 Medium 1577cm -1 The new absorption peak at 1458cm is the stretching vibration absorption peak of the benzene ring skeleton. -1 The absorption peak at is the -CH 2 -CH 2 -In-plane bending vibration absorption peak; at 2957cm -1 and 1410cm -1 、1360cm -1 The methylene groups (-CH 2 -) stretching vibration absorption peak and in-plane bending vibration peak; at 3630~3400cm -1 The peak at 1 is the stretching vibration peak of the hydroxyl group associated between molecules, which belongs to the terminal hydroxyl group in the PBATE copolyester. It can be confirmed that the obtained polyester is PBATE. T represents terephthalic acid Structural unit, A represents adipic acid Structural unit, B represents butanediol -OCH2 CH 2 CH 2 CH 2 O-structural unit, E represents ethylene glycol -OCH 2 CH 2 O-structural unit. Figure 2 It can be seen that the a peak with a chemical shift of δ8.1 is the hydrogen atom peak on the benzene ring of the T structural unit; the j, k, l peaks at δ4.70-4.27 are the hydrogen atom peaks of two methylene groups on the E structural unit; the b, c, d, e peaks at δ4.7-4.1 are the two methylene hydrogen atom peaks connected to the oxygen atom on the B structural unit; the f peak at δ2.32 is the two methylene hydrogen atom peaks connected to the carbonyl group on the A structural unit; the g and h peaks at δ1.80-1.97 are the two middle methylene hydrogen atom peaks on the B structural unit: the i peak at δ1.54-1.66 is the two middle methylene hydrogen atom peaks on the A structural unit. By studying the split peaks of δ=4.70-4.27 and δ=4.43-4.09, the composition ratio of the segments in the copolyester can be calculated and the sequence distribution can be explored. The randomness R=1 indicates that it is a random copolymer, and the molar ratio of the ethylene glycol segment in the polyester is calculated to be 5%.

[0170] According to Examples 1, 5, and 6, it can be seen that when tea polyphenols are used as a chelating agent, compared with phytic acid or stearyl citrate, the poly(ethylene glycol) copolyester has a relatively lower metal ion content, a higher tensile strength, better printing performance, and better biodegradability.

[0171] According to the test results of the comparative examples, in comparative examples 1 and 2, without adding a chelating agent, the metal ions of the obtained multi-copolyesters cannot be effectively removed, the content of metal ions is very high, and the tensile strength of the multi-copolyesters is poor.

[0172] According to the test results of Comparative Examples 3 and 4, it can be seen that in the re-depolymerization process of step S2, when the re-depolymerization temperature is too high or too low, the chelating agent cannot play a good role in removing metal ions, and the metal ion content of the obtained multi-copolyester is still too high; and the crystallinity of the obtained multi-copolyester is also not within the appropriate range, resulting in poor overall performance of the product.

[0173] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A multi-component copolyester, characterized in that: The multi-component copolyester comprises: Component A, a dicarboxylic acid compound, based on the total molar amount of component A, comprises: a1, 35 to 65 mol% of at least one aliphatic dicarboxylic acid; a2, 35 to 65 mol% of at least one aromatic dicarboxylic acid or a derivative thereof; Component B, 1,4-butanediol; Component C, a third monomer, based on the total molar amount of component B and component C, the component C accounts for 5 to 30 mol%; the third monomer is at least one of ethylene glycol, 1,4-cyclohexanedimethanol, and isosorbide; The crystallinity of the multi-component copolyester is 5-22%, the zinc content in the multi-component copolyester is ≤100ppm, the titanium content is ≤120ppm, the calcium content is ≤71ppm, and the silicon content is ≤85ppm.

2. The multi-component copolyester according to claim 1, characterized in that: The melting point of the multi-component copolyester is 105-140°C.

3. The multi-component copolyester according to claim 1, characterized in that: The relative viscosity of the multi-component copolyester is 1.2-1.

8.

4. The multi-component copolyester according to claim 1, characterized in that: The terminal carboxyl content of the multi-component copolyester is 13-30 mmol / t.

5. The multi-component copolyester according to claim 1, characterized in that: The zinc content in the multi-component copolyester is 45-70 ppm, and the titanium content is 50-105 ppm.

6. The multi-component copolyester according to claim 1, characterized in that: The aliphatic dicarboxylic acid is selected from at least one of malonic acid, succinic acid, adipic acid, sebacic acid, pimelic acid, suberic acid, and azelaic acid, and the aromatic dicarboxylic acid or its derivative is selected from at least one of terephthalic acid or its derivative, and isophthalic acid or its derivative.

7. The method for preparing the multi-component copolyester according to any one of claims 1 to 6, characterized in that: The steps include: S1. Initial depolymerization: Dissolving waste terephthalic acid polyester in an alcohol solvent containing a depolymerization catalyst, and carrying out a primary depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions to obtain a primary depolymerization product; The temperature of the initial depolymerization reaction is 180-230°C and the time is 15-120 minutes; S2. Re-depolymerization: Extracting part of the diol from the primary depolymerization product obtained in step S1, adding a chelating agent, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions, and filtering the reactant to obtain a filtrate as the re-depolymerization product; The temperature of the re-depolymerization reaction is 160-190°C and the time is 10-20 minutes; S3. Esterification reaction: According to the monomer content of the multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield is 85-95%, to obtain an esterified product; S4. Polycondensation: After removing excess alcohol solvent from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum until the relative viscosity of the system is 1.2 to 1.8, thereby obtaining the multi-component copolyester.

8. The preparation method according to claim 7, characterized in that: The waste polyester includes one or more of recycled PET, PBT, PET / PBT alloy, and PBAT.

9. The preparation method according to claim 7, characterized in that: At least one of the following (a)-(e): (a) In step S2, the chelating agent includes at least one of stearyl citrate, calcium citrate, tea polyphenols, and phytic acid; preferably tea polyphenols; (b) In step S1, the depolymerization catalyst includes at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate; (c) the polymerization catalyst and the polycondensation catalyst are each independently selected from at least one of butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds, titanium-magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide; (d) the stabilizer is one or more of organic phosphites, trimethyl phosphates, and hindered phenols; (e) The chain extender is at least one of pentaerythritol, trimethylolethane, trimethylolpropane, xylitol, sorbitol, HDI, MDI, TDI, isophorone diisocyanate, ethylene-methyl methacrylate copolymer, and multifunctional epoxy compound ADR.

10. The preparation method according to claim 7, characterized in that: At least one of (f)-(j): (f) In step S2, the chelating agent is added in an amount of 0.01 to 0.1 wt.% of the waste polyester; (g) In step S1, the amount of the depolymerization catalyst added is 0.05 to 0.5 wt.% of the waste polyester; (h) the amount of the chain extender added is 0 to 0.1 wt.% of the waste polyester; (i) In step S4, the amount of the polycondensation catalyst added is 0.03 to 0.1 wt.% of the waste polyester; (j) In step S3, the amount of the polymerization catalyst added is 0.01-0.1 wt.% of the waste polyester.

Citation Information

Patent Citations

  • Synthesis method of poly polyethylene terephthalate-adipate-m-epoxypentadecyl phenol butanediete

    CN112080000A

  • Production device for regenerating recycled polyester into degradable material PBAT

    CN112724388A

  • Biodegradable polyester PBIAT and preparation method thereof

    CN113861399A

  • Method for preparing regenerated polyester by closed-loop recovery of waste polyester with typical green and low-carbon characteristics

    CN114031756A

  • Process for producing polyesters from recycled monomers from pyrolysis and methanol decomposition

    CN114423803A