Polycarbonate oligomer with unsaturated double bond, preparation method thereof, curable composition and preparation method of low-dielectric cured product

The unsaturated double bond polycarbonate oligomer was prepared by alcoholylation and esterification reaction and copolymerization with polyphenylene ether resin, which solved the problem of decreasing molecular weight and difficult to meet electrical properties after polycarbonate recovery, and realized high-frequency circuit board materials Environmentally friendly and efficient use.

CN118930834APending Publication Date: 2024-11-12SWANCOR INNOVATION & INCUBATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310514327.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing polycarbonate recycling technology, physical processing leads to a decrease in molecular weight, deterioration of mechanical properties, chemical recycling requires a large amount of solvents and catalysts, and it is difficult to use recycled plastics on high-end circuit boards; the electrical properties requirements of existing high-frequency circuit board materials High, difficult to meet environmental protection and cost requirements.

Method used

Through alcoholylation and esterification reactions, the waste polycarbonate is prepared as a polycarbonate oligomer with unsaturated double bonds, and copolymerized with polyphenylene ether resin to form a cured product with good heat resistance and electrical properties. Suitable for high-frequency circuit board materials.

Benefits of technology

It realizes the high-value utilization of waste polycarbonate, meets the electrical properties and heat resistance requirements of high-frequency circuit boards, reduces production costs, conforms to environmental protection trends, and provides an environmentally friendly and efficient recycling method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930834A_ABST
    Figure CN118930834A_ABST
Patent Text Reader

Abstract

The invention provides a polycarbonate oligomer with unsaturated double bonds. The polycarbonate oligomer has a structure as shown in a formula (I): # imgabs0 #, wherein each symbol in the formula (I) is defined in the specification. Therefore, the structure does not contain high-polarity alcohol groups, curing can be carried out through free radical polymerization reaction, and application potential is achieved on high-frequency circuit boards and other products. In addition, the polyphenyl ether resin can be copolymerized with currently widely used polyphenyl ether resin, and a cured product can have good electrical characteristics and heat resistance, so that a balanced solution can be provided between development of high-order materials and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polycarbonate oligomer with unsaturated double bonds, a preparation method thereof, a curable composition and a preparation method of a low dielectric curable product, and in particular to a polycarbonate oligomer with unsaturated double bonds that can be copolymerized with a polyphenylene ether resin, a preparation method thereof, a curable composition and a preparation method of a low dielectric curable product. Background Art

[0002] Polycarbonate (PC) is a thermoplastic polymer material formed by ester exchange between bisphenol A and diphenyl carbonate at high temperature. Polycarbonate has good heat resistance and mechanical strength, and is widely used in consumer products such as eyeglass lenses, optical discs, data storage devices, or car lampshades.

[0003] As the use of polycarbonate increases, the issue of polycarbonate recycling has gradually attracted attention. Currently, the recycling of waste polycarbonate products in the market is mostly carried out in the form of physical processing, which is to separate the polycarbonate from the metal parts in the product, and then crush, mix and make other products through high-temperature processes. However, the molecular weight of polycarbonate will decrease during the crushing process, and then the mechanical properties and other physical properties of the recycled product will deteriorate, so its application is still greatly limited.

[0004] Currently, many studies have begun to try to use chemical recycling methods to treat waste polycarbonate products, most of which are to obtain bisphenol A (BPA) monomers through degradation and reuse them in the synthesis of polycarbonate. However, this method requires the use of a large amount of solvents or catalysts and cumbersome purification steps to obtain high-purity bisphenol A. Due to environmental and cost factors, this method is difficult to industrialize.

[0005] In recent years, the demand for consumer electronic products has increased significantly, and the demand for circuit boards has also risen. For example, Japan has a precedent for using polycarbonate in electronic materials (such as publication number TW 202024175A). The aforementioned patent case uses polycarbonate oligomers as epoxy hardeners. After copolymerization, the two can form epoxy resin cured products with good heat resistance and electrical properties. The measured dielectric constant (Dk) of this material is 2.68, and the dielectric loss tangent (Df) is 0.0132, which is a potential material for printed circuit boards.

[0006] In response to the high frequency and high speed requirements of today's high-end circuit boards, NORYLTM SA9000 resin launched by SABIC has gradually become the mainstream. It is a polyphenylene ether (PPE) oligomer with a difunctional unsaturated group at one end. It has good heat resistance and rigidity after free radical polymerization. And because it does not produce polar functional groups after curing, it has a relatively lower dielectric loss tangent and dielectric constant than traditional epoxy resins.

[0007] In view of the rising environmental awareness in various countries, the recycling of plastics is becoming increasingly important. The European Union has also proposed a ban on general plastic products, restricting some plastic products to use a certain amount of recycled plastics. In response to this trend, the above thinking has gradually spread to various chemical products, and brand manufacturers have made advance restrictions on the raw material side. However, the materials used in high-end circuit board products at this stage are difficult to prepare using recycled plastics, and coupled with the product's own requirements for electrical properties, free radical polymerization curing systems have gradually become the mainstream. Based on the above, if waste polycarbonate can be modified into short-chain unsaturated resins, there is a chance to maintain good electrical properties and heat resistance, and in response to future trends, it can be used as one of the recycled raw materials in circuit board materials. Summary of the invention

[0008] The purpose of the present invention is to provide a method for recovering and preparing oligomers from waste polycarbonate. The prepared oligomers have good copolymerization operability with polyphenylene ether materials for high-frequency circuit boards that are widely used in the market today, and have excellent heat resistance and electrical properties after curing, thereby providing the industry with a high-end circuit board material obtained by high-value recycling of raw materials.

[0009] One embodiment of the present invention provides a polycarbonate oligomer having an unsaturated double bond, which has a structure as shown in formula (I):

[0010]

[0011] Wherein, R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8) or formula (9):

[0012]

[0013] Wherein, X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30.

[0014] Another embodiment of the present invention provides a method for preparing the aforementioned polycarbonate oligomer having an unsaturated double bond, comprising the following steps: performing an alcoholysis step, wherein a polycarbonate is dissolved in a reaction solvent, and a first compound and a first catalyst are added thereto and then alcoholysis is performed to obtain a reaction solution of a polycarbonate oligomer having a unilateral unsaturated double bond, wherein the first compound has a structure as shown in formula (II), and the polycarbonate oligomer having a unilateral unsaturated double bond has a structure as shown in formula (III):

[0015]

[0016] An esterification step is performed by adding a second compound and a second catalyst into the reaction solution to perform an esterification reaction to obtain a substance to be purified, wherein the second compound has a structure as shown in formula (IV):

[0017]

[0018] A washing step is performed, wherein the product to be purified is precipitated and washed with an alcohol solvent to form a product to be dried. A drying step is performed, wherein the product to be dried is filtered and dried to obtain a polycarbonate oligomer having an unsaturated double bond. Wherein, R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom, R2 is an alkyl group having 1 to 12 carbon atoms, and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure as shown in formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8) or formula (9):

[0019]

[0020] Wherein, X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30.

[0021] According to the aforementioned preparation method, the molar ratio of the polycarbonate to the first compound may be 1:10 to 1:50.

[0022] According to the aforementioned preparation method, the reaction solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate and cyclohexanone.

[0023] According to the aforementioned preparation method, the first catalyst and the second catalyst can be respectively selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.

[0024] According to the aforementioned preparation method, the molar ratio of the first compound to the first catalyst may be 1:0.002 to 1:0.004.

[0025] According to the aforementioned preparation method, in the alcoholysis step, the polycarbonate and the first compound can undergo alcoholysis reaction at 70° C. to 180° C.

[0026] According to the aforementioned preparation method, the added amount of the first catalyst and the second catalyst may be 10 weight percent to 30 weight percent of the content of the first compound.

[0027] According to the aforementioned preparation method, the molar ratio of the first compound to the second compound may be 1:1 to 1:5.

[0028] According to the aforementioned preparation method, in the esterification step, the polycarbonate oligomer with unilateral unsaturated double bonds and the second compound can be subjected to an esterification reaction at 70° C. to 100° C.

[0029] Another embodiment of the present invention provides a curable composition, which includes the aforementioned polycarbonate oligomer having unsaturated double bonds, a polyphenylene ether resin having unsaturated double bonds, a solvent, and a free radical initiator.

[0030] According to the aforementioned curable composition, the mass ratio of the polycarbonate oligomer having unsaturated double bonds to the polyphenylene ether resin having unsaturated double bonds may be 0.1 to 1.

[0031] According to the aforementioned curable composition, the free radical initiator can be selected from the group consisting of peroxides and azo initiators.

[0032] According to the aforementioned curable composition, the amount of the free radical initiator added may be 0.5 weight percent to 3.0 weight percent of the total content of the polycarbonate oligomer having unsaturated double bonds and the polyphenylene ether resin having unsaturated double bonds.

[0033] According to the aforementioned curable composition, the solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, γ-butyrolactone, butanone, cyclohexanone, toluene and xylene.

[0034] Another embodiment of the present invention provides a method for preparing a low dielectric cured product, wherein the low dielectric cured product is obtained by subjecting the aforementioned curable composition to a curing reaction at a curing temperature, wherein the curing temperature is 140° C. to 250° C.

[0035] Based on this, the present invention proposes a method for recycling and reusing waste polycarbonate, which utilizes the principles of alcoholysis and esterification to prepare a bifunctional polycarbonate oligomer with an unsaturated group at the end. The oligomer can be co-cured with materials commonly used in high-frequency circuit boards. The resulting cured product can have good electrical and physical properties, so that the waste can achieve the goal of recycling and high value while meeting the needs of environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to make the above and other objects, features, advantages and embodiments of the present invention more clearly understood, the accompanying drawings are described as follows:

[0037] Figure 1 The present invention is a flowchart of the steps of preparing the polycarbonate oligomer having unsaturated double bonds.

[0038]

Explanation of symbols

[0039] 100: Preparation method

[0040] 110,120,130,140: Steps DETAILED DESCRIPTION

[0041] The following will discuss various embodiments of the present invention in more detail. However, this embodiment can be an application of various inventive concepts and can be specifically implemented in various specific scopes. The specific embodiments are for illustrative purposes only and are not limited to the scope of the disclosure.

[0042] In the present invention, the compound structure is sometimes represented by a skeleton formula, which may omit carbon atoms, hydrogen atoms, and carbon-hydrogen bonds. If the functional group is clearly drawn in the structural formula, the drawn one shall prevail.

[0043] In the present invention, for the sake of simplicity and fluency, "a first compound having a structure as shown in formula (II)" is sometimes expressed as "a first compound as shown in formula (II)" or "first compound (II)", and the representation of other compounds or groups is similar.

[0044] <Polycarbonate oligomer having unsaturated double bonds>

[0045] One embodiment of the present invention provides a polycarbonate oligomer having an unsaturated double bond, which has a structure as shown in formula (I):

[0046]

[0047] Wherein, R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8) or formula (9):

[0048]

[0049] Wherein, X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30, wherein n represents the degree of polymerization.

[0050] Based on this, the aforementioned polycarbonate oligomer with unsaturated double bonds does not contain a high polar alcohol group in its structure and can be cured by free radical polymerization, which has application potential in products such as high-frequency circuit boards. The polycarbonate oligomer with unsaturated double bonds can be copolymerized with the currently widely used polyphenylene ether resin, and the cured product can have good electrical properties and heat resistance.

[0051] <Method for preparing polycarbonate oligomer having unsaturated double bonds>

[0052] Please refer to Figure 1 , Figure 1 1 is a flow chart of the steps of the method 100 for preparing a polycarbonate oligomer having unsaturated double bonds of the present invention. Another embodiment of the present invention provides a method 100 for preparing a polycarbonate oligomer having unsaturated double bonds, which comprises steps 110, 120, 130 and 140.

[0053] Step 110 is an alcoholysis step, wherein a polycarbonate is dissolved in a reaction solvent, and a first compound and a first catalyst are added thereto to perform an alcoholysis reaction to obtain a reaction solution of a polycarbonate oligomer having a unilateral unsaturated double bond, wherein the first compound has a structure as shown in formula (II), and the polycarbonate oligomer having a unilateral unsaturated double bond has a structure as shown in formula (III):

[0054]

[0055]

[0056] Step 120 is an esterification step, in which a second compound and a second catalyst are added to the reaction solution to perform an esterification reaction to obtain a substance to be purified, wherein the second compound has a structure as shown in formula (IV):

[0057]

[0058] Step 130 is a cleaning step, in which the object to be purified is precipitated and cleaned with an alcohol solvent to form an object to be dried.

[0059] Step 140 is a drying step, in which the product to be dried is filtered and dried to obtain a polycarbonate oligomer having unsaturated double bonds. R1, R2, X, X1, X2, Y, a and n in formula (II), formula (III) and formula (IV) are as defined in the above paragraphs and are not further described here.

[0060] The reaction solvent may be selected from the group consisting of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethylformamide (DMF), anisole, dimethyl sulfoxide (DMSO), propylene glycol methyl ether acetate, propylene glycol methyl ether propionate and cyclohexanone.

[0061] The first catalyst and the second catalyst can be selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) and 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD).

[0062] The molar ratio of the polycarbonate to the first compound may be 1:10 to 1:50, preferably 1:20 to 1:40. The molar ratio of the first compound to the first catalyst may be 1:0.002 to 1:0.004, preferably 1:0.002 to 1:0.003. The amount of the first catalyst and the second catalyst added may be 10 weight percent to 30 weight percent of the content of the first compound, preferably 20 weight percent to 25 weight percent. The molar ratio of the first compound to the second compound may be 1:1 to 1:5, preferably 1:2.2 to 1:4.4.

[0063] The alcoholysis reaction and the esterification reaction can be carried out by heating. In the alcoholysis step, the polycarbonate and the first compound can be subjected to alcoholysis reaction at 70°C to 180°C, preferably at 130°C to 150°C. In the esterification step, the polycarbonate oligomer with unilateral unsaturated double bonds and the second compound can be subjected to esterification reaction at 70°C to 100°C, preferably at 70°C to 90°C.

[0064] For example, if in the polycarbonate oligomer having a unilateral unsaturated double bond represented by the aforementioned formula (III), X has a structure as represented by formula (1), X1, X2 and Y are methyl groups, R1 is a hydrogen atom and R2 is an ethylene group, the prepared polycarbonate oligomer having an unsaturated double bond has a structure as represented by formula (Ia), and the polycarbonate oligomer having a unilateral unsaturated double bond has a structure as represented by formula (III-a):

[0065]

[0066] <Curable Composition>

[0067] Another embodiment of the present invention provides a curable composition, which includes the aforementioned polycarbonate oligomer with unsaturated double bonds, a polyphenylene ether resin with unsaturated double bonds, a solvent and a free radical initiator, and the curable composition can be cured at high temperature to obtain a low dielectric cured product. A mixing sample preparation temperature of the curable composition can be 50°C to 100°C, preferably 70°C to 90°C.

[0068] The free radical initiator can be selected from the group consisting of peroxides and azo initiators, and the solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, γ-butyrolactone, butanone, cyclohexanone, toluene and xylene.

[0069] The mass ratio of the polycarbonate oligomer with unsaturated double bonds to the polyphenylene ether resin with unsaturated double bonds may be 0.1 to 1. The amount of the free radical initiator added may be 0.5 to 3.0 weight percent of the total content of the polycarbonate oligomer with unsaturated double bonds and the polyphenylene ether resin with unsaturated double bonds, preferably 1 to 2.5 weight percent. If the amount of the free radical initiator added is too little, it will lead to incomplete curing, resulting in a decrease in the physical properties of the curable composition, and if it is added too much, the electrical properties of the curable composition will be decreased.

[0070] <Method for preparing low dielectric cured product>

[0071] Another embodiment of the present invention provides a method for preparing a low dielectric cured product, which is obtained by subjecting the aforementioned curable composition to a curing reaction at a curing temperature, wherein the curing temperature is 140°C to 250°C, preferably 180°C to 220°C, but not limited thereto. Technicians in the technical field of the present invention can select an appropriate curing temperature, such as 140°C to 180°C, 140°C to 220°C, 150°C to 250°C, etc.

[0072] The present invention is further illustrated by the following specific examples, which are used to facilitate those skilled in the art to which the present invention belongs, so that they can fully utilize and practice the present invention without excessive interpretation. These examples should not be regarded as limiting the scope of the present invention, but are used to illustrate how to implement the materials and methods of the present invention.

[0073] <Preparation of polycarbonate oligomer having unsaturated double bonds>

[0074] <Example 1>

[0075] Take 100 g (4×10 -3 mole (calculated as Mn) of polycarbonate ester pellets (purchased from Chi Mei Industrial, product code PC-122, Mn=24400, Mw=45488) were completely dissolved in 150 g of DMAc at 150°C, and 10.07 g (0.082 mole) of hydroxyethyl methacrylate was added dropwise to the above solution. After uniform mixing, 0.026 g (1.69×10 -4 mole) of DBU, react for 5 hours, cool down after reaction, pour into methanol for cleaning, filter by suction, and dry in a vacuum oven at 78°C to obtain a compound as shown in formula (III-a), the product code is HEPC, the yield is about 71%, and the product can be analyzed by GPC to obtain Mn=2721, Mw=4061.

[0076] <Example 2>

[0077] The first half of the steps were the same as those in Example 1, except that after the reaction was completed, the mixture was not washed with methanol. The temperature was lowered to 70° C., and 2.33 g (22 weight percent of the content of the first compound (II)) of DBU and 27.81 g (0.180 mole) of methacrylic anhydride were added in sequence. The mixture was reacted at 70° C. for 6 hours. After the reaction was completed, the mixture was washed with methanol, filtered, and dried in a vacuum oven at 78° C. to obtain a white powder of formula (Ia). The product code was HAPC-1, and the yield was about 73.6%. GPC analysis of the product showed that Mn=2366 and Mw=4137.

[0078] <Example 3>

[0079] Take 100 g (4×10-3 mole (calculated as Mn) of polycarbonate ester pellets (purchased from Chi Mei Industrial, product code PC-122, Mn=24400, Mw=45488) were completely dissolved in 150 g of DMAc at 150°C, and then 16.51 g (0.127 mole) of hydroxyethyl methacrylate was added dropwise to the above solution. After uniform mixing, 0.038 g (2.54×10 -4 The mixture was reacted for 5 hours. After that, the temperature was lowered to 70°C and 3.63 g (22 weight percent of the first compound (II)) of DBU and 43.03 g (0.279 mole) of methacrylic anhydride were added in sequence. The mixture was reacted for 6 hours at 78°C. After that, the mixture was washed with methanol, filtered by suction, and dried in a vacuum oven at 78°C to obtain a white powder of formula (Ia). The product code was HAPC-1.5. The yield was about 59%. GPC analysis of the product showed that Mn=2673 and Mw=4479.

[0080] <Example 4>

[0081] Take 100 g (3.8 × 10 -3 mole, calculated as Mn) of recycled polycarbonate ester pellets (purchased from Chi Mei Industrial, product code GC-122B, Mn=26099, Mw=47827) were completely dissolved in 150 g of DMAc at 150°C, and then 14.97 g (0.115 mole) of hydroxyethyl methacrylate was added dropwise to the above solution, mixed evenly, and then 0.035 g (2.30×10 - 4 The mixture was reacted for 5 hours. After the reaction, the temperature was lowered to 70°C and 3.29 g (22 weight percent of the first compound (II)) of DBU and 39.00 g (0.253 mole) of methacrylic anhydride were added in sequence. The mixture was reacted at 80°C for 6 hours. After the reaction, the mixture was washed with methanol, filtered and dried in a vacuum oven at 78°C to obtain a gray powder of formula (Ia). The product code was HAGC-1.5. The yield was about 70.7%. GPC analysis of the product showed that Mn=2658 and Mw=4885.

[0082] <Example 5>

[0083] Take 100 g (3.8 × 10 -3mole, calculated as Mn) of recycled polycarbonate ester pellets (purchased from Chi Mei Industrial, product code GC-122B, Mn=26099, Mw=47827) were completely dissolved in 150 g of DMAc at 150°C, and then 19.91 g (0.153 mole) of hydroxyethyl methacrylate was added dropwise to the above solution, mixed evenly, and then 0.046 g (3.02×10 - 4 The mixture was reacted for 5 hours. After the reaction, the temperature was lowered to 80°C and 4.38 g (22 weight percent of the first compound (II)) of DBU and 51.89 g (0.337 mole) of methacrylic anhydride were added in sequence. The mixture was reacted at 80°C for 6 hours. After the reaction, the mixture was washed with methanol, filtered and dried in a vacuum oven at 78°C to obtain a gray powder of formula (Ia). The product code was HAGC-2. The yield was about 61.9%. GPC analysis of the product showed that Mn=2257 and Mw=4445.

[0084] <Comparative Example 1>

[0085] Take 100 g (4×10 -3 150 g of DMAc was dissolved in 150 g of polycarbonate ester pellets (purchased from Chi Mei Industrial, product code PC-122, Mn=24400, Mw=45488) and heated to 120°C for dissolution. After dissolution, 7.28 g (0.0846 mole) of methacrylic acid and 0.129 g (2.47 mole) of DBU were added dropwise. The reaction was continued for 3 hours. After the reaction was completed, the reaction mixture was cooled and poured into methanol for washing, filtered by vacuum extraction, and dried in a vacuum oven at 78°C to obtain a white powder. The product code was MAPC. The solubility of the obtained product in organic solvents was poor. It was speculated that free radical crosslinking reaction had occurred during the reaction and further operation and analysis were impossible.

[0086] <Curing Reaction of Curable Composition>

[0087] The aforementioned polycarbonate oligomer having unsaturated double bonds can be further prepared into a curable composition and subjected to a curing reaction. Specifically, the aforementioned polycarbonate oligomer having unsaturated double bonds, a polyphenylene ether resin having unsaturated double bonds, a solvent and a free radical initiator can be mixed to obtain a curable composition, whereby the polycarbonate oligomer, the polyphenylene ether resin, the solvent and the free radical initiator can form a prepolymer containing the curable composition, the details of which are as described in the aforementioned paragraph and will not be repeated here.

[0088] Next, the polycarbonate oligomer with unsaturated double bonds and the polyphenylene ether resin can be cross-linked and cured under the catalysis of a free radical initiator, and the curing reaction can be completed by heating the curable composition. Specific examples are provided below for illustration.

[0089] <Example 6>

[0090] Take 0.24 g of polycarbonate oligomer HAPC-1 with unsaturated double bonds and 0.96 g of polyphenylene ether resin NORYL TM SA9000 (purchased from SABIC) was dissolved in 2.856 g of cyclohexanone, heated and mixed at 80°C, and then 0.024 g (2.0 weight percent of the total content of polycarbonate oligomer and polyphenylene ether resin) of diisopropylbenzene peroxide was added as a free radical initiator. After stirring evenly, a mixed prepolymer was obtained, which was placed in an oven at 80°C for 12 hours to bake out part of the solvent. The subsequent curing reaction was gradually heated from 140°C to 220°C to obtain a low dielectric cured product.

[0091] <Example 7>

[0092] The preparation steps of Example 7 are the same as those of Example 6, except that the amount of the polycarbonate oligomer HAPC-1 having an unsaturated double bond is changed to 0.36 g, and the polyphenylene ether resin NORYL TM The dosage of SA9000 was changed to 0.84 g.

[0093] <Example 8>

[0094] The preparation steps of Example 8 are the same as those of Example 6, except that the amount of the polycarbonate oligomer HAPC-1 having an unsaturated double bond is changed to 0.48 g, and the polyphenylene ether resin NORYL TM The dosage of SA9000 was changed to 0.72 g.

[0095] <Example 9>

[0096] The preparation steps of Example 9 are the same as those of Example 6, except that the amount of the polycarbonate oligomer HAPC-1 having an unsaturated double bond is changed to 0.60 g, and the polyphenylene ether resin NORYL TM The dosage of SA9000 was changed to 0.60 g.

[0097] <Comparative Example 2>

[0098] Take 0.24 g of polycarbonate oligomer HEPC with unsaturated double bonds and 0.96 g of polyphenylene ether resin NORYL TMSA9000 (purchased from SABIC) was dissolved in 2.856 g of cyclohexanone, heated and mixed at 80°C, and then 0.024 g (2.0 weight percent of the total content of polycarbonate oligomer and polyphenylene ether resin) of diisopropylbenzene peroxide was added as a free radical initiator, and stirred evenly to obtain a mixed prepolymer, which was placed in an oven at 80°C for 12 hours to bake out part of the solvent, and then the temperature was gradually raised from 140°C to 220°C for the subsequent curing reaction. After the curing reaction, the product of Comparative Example 2 had severe shrinkage and phase separation.

[0099] <Comparative Example 3>

[0100] The preparation steps of Comparative Example 3 are the same as those of Comparative Example 2, except that the amount of the polycarbonate oligomer HEPC having an unsaturated double bond is changed to 0.36 g, and the polyphenylene ether resin NORYL TM The amount of SA9000 was changed to 0.84 g. After the curing reaction, the product of Comparative Example 3 had serious shrinkage and phase separation.

[0101] <Comparative Example 4>

[0102] The preparation steps of Comparative Example 4 are the same as those of Comparative Example 2, except that the amount of the polycarbonate oligomer HEPC having an unsaturated double bond is changed to 0.48 g, and the polyphenylene ether resin NORYL TM The amount of SA9000 was changed to 0.72 g. After the curing reaction, the product of Comparative Example 4 had serious shrinkage and phase separation.

[0103] <Comparative Example 5>

[0104] The preparation steps of Comparative Example 5 are the same as those of Comparative Example 2, except that the amount of the polycarbonate oligomer HEPC having an unsaturated double bond is changed to 0.60 g, and the polyphenylene ether resin NORYL TM The amount of SA9000 was changed to 0.60 g. After the curing reaction, the product of Comparative Example 5 had serious shrinkage and phase separation.

[0105] <Testing the properties of low dielectric cured products>

[0106] The low dielectric cured products obtained in Examples 6 to 9 were measured by differential scanning calorimeter (DSC) to determine the glass transition temperature (T g ) were measured at a heating rate of 10°C / min, and the measurement results are listed in Table 1 below.

[0107]

[0108] According to the above results, the polycarbonate oligomer with unsaturated double bonds synthesized by the present invention does have good reactivity with the polyphenylene ether resin, can react and cure under the above oven conditions, has good compatibility and film-forming properties, and is easy to operate and process. In addition, the polycarbonate oligomer with unsaturated double bonds of the present invention can be used in combination with the polyphenylene ether resin in the above ratio.

[0109] Furthermore, in terms of heat resistance, the glass transition temperature decreases as the amount of polycarbonate oligomers with unsaturated double bonds added increases, but it can still maintain good heat resistance, which is sufficient to meet various application requirements.

[0110] The following will further conduct electrical tests on the low dielectric cured products of Examples 6 to 9 to obtain their dielectric properties. The frequency used in the test is 10 GHz, and the dielectric constant (D k ) and dielectric loss tangent (D f ) are listed in Table 2 below.

[0111]

[0112] According to the above experimental results, compared with the SA9000 cured product cured by pure polyphenylene ether resin, the low dielectric cured product cured by adding the polycarbonate oligomer with unsaturated double bonds synthesized by the present invention has better D k Performance, but in D f In addition, it can be seen from the above results that as the amount of polycarbonate oligomer with unsaturated double bonds increases, the dielectric properties of the low dielectric curing material can be further improved, making D f Return to the best performance, and obtain better D than SA9000 cured product k The performance shows the potential of the low dielectric cured product of the present invention in high frequency applications.

[0113] In summary, the present invention provides a method for recycling and reusing waste polycarbonate, which is to use a monool compound containing a double bond structure to perform alcoholysis on polycarbonate, and after the polycarbonate is prepared into an oligomer, the residual terminal phenol group is modified to obtain a polycarbonate oligomer with unsaturated double bonds, and the ends of the polycarbonate oligomers have unsaturated double bonds. The polycarbonate oligomers with unsaturated double bonds are compatible with polyphenylene ether resins in organic solvents, and the two can be cured by free radical polymerization to prepare samples. During the sample preparation process, the ratio of polycarbonate oligomers with unsaturated double bonds and polyphenylene ether resins can be adjusted to achieve the desired physical and electrical properties, and the resulting low-dielectric cured product can have good dielectric loss tangent and dielectric constant performance, and is expected to be implemented on high-frequency circuit board materials.

[0114] The above embodiments are only for illustrating the principles of the present invention and are not intended to limit the scope thereof. For example, other alcohols or polycarbonate resins may be used and polycarbonate oligomers with unsaturated double bonds of different chemical structures may be prepared through similar reactions. Therefore, any modification or extension of the above embodiments shall fall within the scope of the present invention.

Claims

1. A polycarbonate oligomer having unsaturated double bonds, characterized in that: The polycarbonate oligomer having unsaturated double bonds has a structure as shown in formula (I): Wherein, R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8) or formula (9): Wherein, X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; wherein Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30.

2. A method for preparing a polycarbonate oligomer having unsaturated double bonds as claimed in claim 1, characterized in that: Include: The alcoholysis step is to dissolve a polycarbonate in a reaction solvent, add a first compound and a first catalyst, and then perform alcoholysis reaction to obtain a reaction solution of a polycarbonate oligomer having a unilateral unsaturated double bond, wherein the first compound has a structure as shown in formula (II), and the polycarbonate oligomer having a unilateral unsaturated double bond has a structure as shown in formula (III): An esterification step is performed by adding a second compound and a second catalyst into the reaction solution to perform an esterification reaction to obtain a substance to be purified, wherein the second compound has a structure as shown in formula (IV): Performing a washing step, which is to wash the object to be purified by precipitation with an alcohol solvent to form an object to be dried; and Performing a drying step, filtering and drying the substance to be dried to obtain the polycarbonate oligomer having unsaturated double bonds; Wherein, R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8) or formula (9): Wherein, X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; wherein Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the polycarbonate to the first compound is 1:10 to 1:

50.

4. The preparation method according to claim 2, characterized in that: The reaction solvent is selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate and cyclohexanone.

5. The preparation method according to claim 2, characterized in that: The first catalyst and the second catalyst are respectively selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.

6. The preparation method according to claim 2, characterized in that: The molar ratio of the first compound to the first catalyst is 1:0.002 to 1:0.

004.

7. The preparation method according to claim 2, characterized in that: In the alcoholysis step, the polycarbonate and the first compound undergo an alcoholysis reaction at 70° C. to 180° C.

8. The preparation method according to claim 2, characterized in that: The added amount of the first catalyst and the second catalyst is 10 weight percent to 30 weight percent of the content of the first compound.

9. The preparation method according to claim 2, characterized in that: The molar ratio of the first compound to the second compound is 1:1 to 1:

5.

10. The preparation method according to claim 2, characterized in that: In the esterification step, the polycarbonate oligomer having a unilateral unsaturated double bond and the second compound are subjected to an esterification reaction at 70° C. to 100° C.

11. A curable composition, characterized in that The curable composition comprises the polycarbonate oligomer having unsaturated double bonds as claimed in claim 1 , a polyphenylene ether resin having unsaturated double bonds, a solvent and a free radical initiator.

12. The curable composition according to claim 11, wherein The mass ratio of the polycarbonate oligomer having unsaturated double bonds to the polyphenylene ether resin having unsaturated double bonds is 0.1 to 1.

13. The curable composition according to claim 11, wherein The free radical initiator is selected from the group consisting of peroxides and azo initiators.

14. The curable composition according to claim 11, wherein The added amount of the free radical initiator is 0.5 weight percent to 3.0 weight percent of the total content of the polycarbonate oligomer having unsaturated double bonds and the polyphenylene ether resin having unsaturated double bonds.

15. The curable composition according to claim 11, wherein The solvent is selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, γ-butyrolactone, butanone, cyclohexanone, toluene and xylene.

16. A method for preparing a low dielectric cured product, characterized in that: A low dielectric cured product is obtained by subjecting the curable composition as claimed in claim 11 to a curing reaction at a curing temperature, wherein the curing temperature is 140° C. to 250° C.