Polyethylene glycol monoricinoleate as well as preparation method and application thereof

By adding water azeotropic agent and silicone modifier to the esterification reaction of polyethylene glycol monoricinoleate, the problems of dark color and poor performance of the product are solved, and low color and high dynamic color are achieved Index coating products improve the performance and effectiveness of coatings.

CN118930840AActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411200026.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing polyethylene glycol monoricinoleate products have dark colors and poor performance, which affects the paint finish and dynamic color index of the paint.

Method used

In the presence of an acid catalyst, polyethylene glycol and ricinoleic acid are used as raw materials, and a water azeotrope and a silicone modifier are added for esterification and synthesis. The system electron cloud density and free radical reaction are reduced by siloxane modifier. , improve thermal stability performance, and remove water in the esterification reaction through a water azeotrope to stabilize the reaction process.

Benefits of technology

Low-color, high-quality polyethylene glycol monoricinoleate products are obtained, which can significantly improve the dynamic color index and performance of the paint as a coating additive.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of organic synthesis, particularly relates to a preparation method of polyethylene glycol monorricinoleate, particularly relates to low-chroma polyethylene glycol monorricinoleate, and further discloses a preparation method and application of the low-chroma polyethylene glycol monorricinoleate. According to the preparation method of the polyethylene glycol monorricinoleate, based on a traditional esterification reaction system, polyethylene glycol and ricinoleic acid are used as raw materials, organic acid or inorganic acid is used as a catalyst, and esterification is carried out to obtain the polyethylene glycol monorricinoleate. By adding the water entrainer and the siloxane modifier into a reaction system, the problems of dark color and poor performance of the product in the prior art are solved, and particularly, the water entrainer can be used as a coating additive to obtain a coating product with a high dynamic color index.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic synthesis, and specifically relates to a preparation method of polyethylene glycol monoricinoleate, in particular to low-chroma polyethylene glycol monoricinoleate, and further discloses the preparation method and application thereof. Background Art

[0002] In recent years, with the improvement of people's living standards and the enhancement of environmental awareness, the use of biomass such as natural plant oils as raw materials to develop new green surfactants with low toxicity and biodegradability has become an industry development trend. Polyethylene glycol monoricinoleate is a non-ionic surfactant that can be used to disperse pigments, pearlescent agents, etc. in the production process of water-based coating systems, printing inks and thermoplastics. It can promote the deflocculation of pigments. Since the particle size of the deflocculated pigment is small, it can not only improve the gloss of the coating and enhance the color intensity, but also improve the transparency of transparent pigments and the hiding power of opaque pigments. At present, industrial paints and coatings with polyethylene glycol monoricinoleate are mainly used in the fields of construction, automobiles, cans, leather, etc.

[0003] Studies have shown that polyethylene glycol monoricinoleate as a coating additive also has an important influence on the final glittering effect of the paint surface. At present, the strength of the paint surface glittering effect is often expressed by the dynamic color index, and the color number, purity, acid value, etc. of polyethylene glycol monoricinoleate itself will ultimately affect the dynamic color index. However, the traditional synthesis process of polyethylene glycol monoricinoleate mainly adopts the direct esterification method, that is, it uses catalysts such as sulfuric acid, p-toluenesulfonic acid, boric acid, solid acid, etc. to obtain it by direct esterification under high temperature conditions. The polyethylene glycol monoricinoleate products prepared under this process are mostly amber or dark yellow, and the product color is often darker, which affects the paint effect of subsequent coating products.

[0004] For example, Chinese patent CN102816324A reports a method for synthesizing polyethylene glycol monoricinoleate by borate method, wherein polyethylene glycol and boric acid are reacted to generate borate, and then PTS catalyst is added to ricinoleic acid for esterification, and the product obtained by esterification is a light yellow liquid. For another example, the document "Research and Development of Synthesis Process of Low-Chroma Polyethylene Glycol 400 Dioleate" reports the use of oleic acid and polyethylene glycol 400 under catalyst conditions, and the use of antioxidant X as a protective agent to carry out the synthesis process of polyethylene glycol dioleate, and a product with a chromaticity of 150APHA can be obtained. Therefore, this field expects to develop more low-chroma, high-performance polyethylene glycol monoricinoleate products, which has positive significance for preparing coating products with high dynamic color index. Summary of the invention

[0005] To this end, the technical problem to be solved by the present invention is to provide a method for preparing polyethylene glycol monoricinoleate, so as to solve the problem that the polyethylene glycol monoricinoleate product in the prior art has dark color and poor performance;

[0006] The second technical problem to be solved by the present invention is to improve the polyethylene glycol monoricinoleate prepared by the above method and its application. The polyethylene glycol monoricinoleate can be used as a coating additive to obtain a coating product with a high dynamic color index.

[0007] In order to solve the above technical problems, the preparation method of polyethylene glycol monoricinoleate described in the present invention comprises the steps of esterification synthesis in the presence of an acidic catalyst, using polyethylene glycol and ricinoleic acid as raw materials, and adding a water entrainer and a siloxane modifier.

[0008] Specifically, in the preparation method of polyethylene glycol monoricinoleate, the siloxane modifier includes one or a mixture of hexamethyldisiloxane, octamethyltrisiloxane, hexaethyldisiloxane, hexaphenyldisiloxane, methyloctadecanoylsiloxane or tetradecamethylhexasiloxane;

[0009] Preferably, the siloxane modifier comprises hexaphenyldisiloxane and / or hexamethyldisiloxane.

[0010] Specifically, in the preparation method of polyethylene glycol monoricinoleate, the amount of the siloxane modifier added is 1-20wt% of the mass of the ricinoleic acid;

[0011] Preferably, the added amount of the siloxane modifier is 5-10 wt % of the mass of the ricinoleic acid.

[0012] Specifically, in the preparation method of polyethylene glycol monoricinoleate, the water entrainer includes an organic solvent that can form an azeotrope with water;

[0013] Preferably, the water entrainer comprises one or a mixed solvent of n-hexane, cyclohexane, n-heptane, n-octane, toluene, benzene, xylene or n-decane;

[0014] Preferably, the water entrainer comprises n-heptane and / or n-octane.

[0015] Specifically, in the preparation method of polyethylene glycol monoricinoleate, the molar ratio of the polyethylene glycol to the ricinoleic acid is 1.0-1.5:1.

[0016] Specifically, in the preparation method of polyethylene glycol monoricinoleate, the polyethylene glycol includes one or a mixture of polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, polyethylene glycol-1000, polyethylene glycol-2000 or polyethylene glycol-5000;

[0017] Preferably, the polyethylene glycol includes one of polyethylene glycol-400, polyethylene glycol-600 or polyethylene glycol-800 or a mixture of several thereof.

[0018] Specifically, in the method for preparing polyethylene glycol monoricinoleate, the acidic catalyst includes at least one of an organic acid catalyst or an inorganic acid catalyst;

[0019] Preferably, the acidic catalyst comprises one or a mixture of sulfuric acid, acetic acid, p-toluenesulfonic acid, methanesulfonic acid, benzoic acid or phenylacetic acid;

[0020] Preferably, the acidic catalyst comprises methanesulfonic acid and / or p-toluenesulfonic acid;

[0021] Preferably, the amount of the acidic catalyst is 0.1-2.0wt% of the mass of the ricinoleic acid. In the esterification process of the present invention, the amount of the acidic catalyst has a certain influence on the chromaticity of the polyethylene glycol monoricinoleate product. Usually, when the amount of the acidic catalyst exceeds 5%, the color number of the system will be deepened, which is difficult to meet the product requirements.

[0022] Specifically, the preparation method of polyethylene glycol monoricinoleate is:

[0023] The temperature of the esterification reaction is 100-200°C, preferably 120-160°C; and / or,

[0024] The reaction time of the esterification reaction is 2-24h.

[0025] Specifically, the method for preparing polyethylene glycol monoricinoleate further comprises the steps of collecting the esterification reaction product and removing the azeotrope formed by the water entrainer and water.

[0026] The invention also discloses polyethylene glycol monoricinoleate prepared by the method.

[0027] The invention also discloses the use of the polyethylene glycol monoricinoleate in preparing a high dynamic color index coating product, in particular, in preparing a coating additive.

[0028] The preparation method of polyethylene glycol monoricinoleate of the present invention is based on a traditional esterification reaction system, using polyethylene glycol and ricinoleic acid as raw materials, using an organic acid or an inorganic acid as a catalyst to esterify polyethylene glycol monoricinoleate. By adding a water entrainer and a siloxane modifier to the reaction system, the problem of deep color and poor performance of the prior art products is solved, especially as a coating additive, a coating product with a high dynamic color index can be obtained.

[0029] The preparation method of polyethylene glycol monoricinoleate of the present invention adds siloxane as a modifier, especially a siloxane modifier containing phenyl or alkyl, on the basis of a traditional esterification reaction. During the esterification synthesis process, the phenyl or alkyl contained in the siloxane can generate a coordination structure with Si atoms, that is, a dπ-pπ coordination bond can be formed in Si-C, so that the electron cloud density of the system is reduced, the energy of the system is reduced, the reaction of free radicals can be blocked, and the thermal stability of the system is improved; moreover, the added siloxane can improve the thermal sensitivity of the system, and even if it is heated for a long time, it can ensure that the undesirable components are controlled at an extremely low level, thereby ensuring the product quality.

[0030] The preparation method of polyethylene glycol monoricinoleate of the present invention can effectively remove water produced in the esterification reaction by adding a water entrainer, especially an organic solvent that can form an azeotrope with water on the basis of a traditional esterification reaction, and effectively ensure the stability of the entire esterification process. After the reaction is completed, the azeotrope of the water entrainer and water can be simply removed to obtain a low-color-number, high-quality polyethylene glycol monoricinoleate product, so as to meet the requirements of high-performance, low-color-number products, effectively solve the problems of dark color and poor performance of products in the prior art, and especially can obtain a coating product with a high dynamic color index as a coating additive. DETAILED DESCRIPTION

[0031] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0032] In the following embodiment of the present invention, in order to improve the chromaticity and application performance of polyethylene glycol monoricinoleate products, a method for preparing polyethylene glycol monoricinoleate is provided, which includes the steps of esterification synthesis in the presence of an acidic catalyst, using polyethylene glycol and ricinoleic acid as raw materials, and adding a water entrainer and a siloxane modifier.

[0033] The preparation method of polyethylene glycol monoricinoleate of the present invention can effectively remove water generated in the esterification reaction by adding a siloxane modifier and a water entrainer on the basis of a traditional esterification reaction, thereby effectively ensuring the stability of the entire esterification process. After the reaction is completed, the azeotrope of the water entrainer and water is simply removed to obtain a low-color-number, high-quality polyethylene glycol monoricinoleate product, thereby meeting the requirements of high-performance, low-color-number products, effectively solving the problems of dark color and poor performance of products in the prior art, and in particular, as a coating additive, a coating product with a high dynamic color index can be obtained.

[0034] As some practicable embodiments, the siloxane modifier includes one or a mixture of hexamethyldisiloxane, octamethyltrisiloxane, hexaethyldisiloxane, hexaphenyldisiloxane, methyloctadecanoylsiloxane or tetradecamethylhexasiloxane;

[0035] Preferably, the siloxane modifier comprises hexaphenyldisiloxane and / or hexamethyldisiloxane.

[0036] The preparation method of polyethylene glycol monoricinoleate of the present invention adds siloxane as a modifier, especially a siloxane modifier containing phenyl or alkyl, on the basis of a traditional esterification reaction. During the esterification synthesis process, the phenyl or alkyl contained in the siloxane can generate a coordination structure with Si atoms, that is, a dπ-pπ coordination bond can be formed in Si-C, so that the electron cloud density of the system is reduced, the energy of the system is reduced, the reaction of free radicals can be blocked, and the thermal stability of the system is improved; moreover, the added siloxane can improve the thermal sensitivity of the system, and even if it is heated for a long time, it can ensure that the undesirable components are controlled at an extremely low level, thereby ensuring the product quality.

[0037] As some practicable methods, the amount of the silicone modifier added is 1-20wt% of the mass of the ricinoleic acid;

[0038] Preferably, the added amount of the siloxane modifier is 5-10 wt % of the mass of the ricinoleic acid.

[0039] As some practicable embodiments, the water entrainer includes a mixed solvent of one or more of n-hexane, cyclohexane, n-heptane, n-octane, toluene, benzene, xylene or n-decane;

[0040] Preferably, the water entrainer comprises n-heptane and / or n-octane.

[0041] As some practicable embodiments, the molar ratio of the polyethylene glycol to the ricinoleic acid is 1.0-1.5:1.

[0042] As some practicable embodiments, the polyethylene glycol includes one or a mixture of polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, polyethylene glycol-1000, polyethylene glycol-2000 or polyethylene glycol-5000;

[0043] Preferably, the polyethylene glycol includes one of polyethylene glycol-400, polyethylene glycol-600 or polyethylene glycol-800 or a mixture of several thereof.

[0044] As some practicable embodiments, the acidic catalyst includes at least one of an organic acid catalyst or an inorganic acid catalyst;

[0045] Preferably, the acidic catalyst comprises one or a mixture of sulfuric acid, acetic acid, p-toluenesulfonic acid, methanesulfonic acid, benzoic acid or phenylacetic acid;

[0046] Preferably, the acidic catalyst comprises methanesulfonic acid and / or p-toluenesulfonic acid.

[0047] As some practicable methods, the amount of the acidic catalyst is 0.1-2.0wt% of the mass of the ricinoleic acid. In the esterification process of the present invention, the amount of the acidic catalyst has a certain influence on the chromaticity of the polyethylene glycol monoricinoleate product. Generally, when the amount of the acidic catalyst exceeds 5%, the color number of the system will be deepened, which is difficult to meet the product requirements.

[0048] As some practicable modes, the temperature of the esterification reaction is 100-200°C, preferably 120-160°C;

[0049] As some practicable embodiments, the reaction time of the esterification reaction is 2-24 hours.

[0050] As some practicable embodiments, the method further comprises the steps of collecting the esterification reaction product and removing the azeotrope formed by the water entrainer and water.

[0051] The invention also discloses polyethylene glycol monoricinoleate prepared by the method.

[0052] The invention also discloses the use of the polyethylene glycol monoricinoleate in preparing a high dynamic color index coating product, in particular, in preparing a coating additive.

[0053] In the following examples of the present invention, chromatographic method is used to monitor and verify the products during the entire esterification process.

[0054] As an exemplary detection method, the gas chromatography parameters in the following embodiments of the present invention are as follows:

[0055] Gas chromatograph: Agilent 7820A;

[0056] Chromatographic column HP-5 (30m×320μm×0.25μm);

[0057] Inlet temperature: 150°C;

[0058] Split ratio 50:1;

[0059] Carrier gas flow rate: 1.5ml / min;

[0060] Heating program: 50 °C for 1 min, increase the temperature to 90 °C at 10 °C / min, hold for 0 min, then increase the temperature to 180 °C at 5 °C / min, hold for 0 min, then increase the temperature to 280 °C at 30 °C / min, hold for 6 min;

[0061] Detector temperature: 280°C.

[0062] Example 1

[0063] Take a three-necked flask equipped with a stirrer, a water separator and a condenser and connect a double-row tube for inert gas protection, add ricinoleic acid (1 mol), polyethylene glycol-600 (1.1 mol), n-octane (300.0 g), hexaphenyldisiloxane (5 wt% of the mass of ricinoleic acid) and 3.0 g of p-toluenesulfonic acid (1.0 wt% of the mass of ricinoleic acid) into the three-necked flask and mix thoroughly.

[0064] Turn on the stirring blade and control the oil bath heating, keep the reaction temperature at about 140°C, and heat for 8 hours. After the reaction, stop heating when water is separated from the water separator. Perform reduced pressure distillation on the collected reaction solution at 140°C and a vacuum degree of 10KPa to remove the azeotrope of n-octane and water to obtain polyethylene glycol monoricinoleate.

[0065] In this embodiment, the reaction product was detected by gas chromatography and the structure was correct.

[0066] In this embodiment, the conversion rate and selectivity of the reaction target product are measured respectively; wherein the conversion rate refers to the percentage of the molar amount of ricinoleic acid converted to the initial molar amount of ricinoleic acid; and the selectivity refers to the ratio of the ricinoleic acid consumed in the production of polyethylene glycol monoricinoleate to the total ricinoleic acid consumed.

[0067] In this embodiment, the conversion rate of the target product was measured to be 99.4%, and the selectivity of polyethylene glycol monoricinoleate was 95.3%.

[0068] Example 2

[0069] Take a three-necked flask equipped with a stirrer, a water separator and a condenser and connect a double-row tube for inert gas protection, add ricinoleic acid (1 mol), polyethylene glycol-600 (1.05 mol), cyclohexane (300.0 g), hexaphenyldisiloxane (accounting for 6.7 wt% of the mass of ricinoleic acid) and p-toluenesulfonic acid (accounting for 0.7 wt% of the mass of ricinoleic acid) into the three-necked flask and mix thoroughly.

[0070] The stirring blade was turned on and the oil bath was controlled to heat, the reaction temperature was maintained at about 120°C, and the heating was continued for 16 hours. The heating was stopped when water was separated in the water separator after the reaction. The collected reaction solution was subjected to reduced pressure distillation at 120°C and a vacuum degree of 5KPa to remove the azeotrope of cyclohexane and water, and polyethylene glycol monoricinoleate was obtained.

[0071] In this embodiment, the reaction product was detected by gas chromatography and the structure was correct. The conversion rate of the target product was determined to be 99.6%, and the selectivity of polyethylene glycol monoricinoleate was 95.7%.

[0072] Example 3

[0073] Take a three-necked flask equipped with a stirrer, a water separator and a condenser and connect a double-row tube for inert gas protection, add ricinoleic acid (1 mol), polyethylene glycol-400 (1 mol), cyclohexane (300.0 g), hexamethyldisiloxane (5 wt% of the mass of ricinoleic acid) and phenylacetic acid (0.5 wt% of the mass of ricinoleic acid) into the three-necked flask and mix thoroughly.

[0074] The stirring blade was turned on and the oil bath was controlled to heat, the reaction temperature was maintained at about 160°C, and the heating was continued for 10 hours. After the reaction, the heating was stopped when water was separated from the water separator. The collected reaction solution was subjected to reduced pressure distillation at 140°C and a vacuum degree of 10 KPa to remove the azeotrope of cyclohexane and water, and polyethylene glycol monoricinoleate was obtained.

[0075] In this embodiment, the reaction product was detected by gas chromatography and the structure was correct. The conversion rate of the target product was 95.3% and the selectivity of polyethylene glycol monoricinoleate was 90.4%.

[0076] Example 4

[0077] Take a three-necked flask equipped with a stirrer, a water separator and a condenser and connect a double-row tube for inert gas protection, add ricinoleic acid (1 mol), polyethylene glycol-800 (1.2 mol), n-heptane (300.0 g), octamethyltrisiloxane (accounting for 10 wt% of the mass of ricinoleic acid) and sulfuric acid (accounting for 1.0 wt% of the mass of ricinoleic acid) into the three-necked flask and mix thoroughly.

[0078] The stirring blade is turned on and the oil bath is controlled to heat, the reaction temperature is maintained at about 100°C, and the heating is carried out for 24 hours. After the reaction, when water is separated from the water separator, the heating is stopped. The collected reaction solution is subjected to reduced pressure distillation at 140°C and a vacuum degree of 10 KPa to remove the azeotrope of n-heptane and water to obtain polyethylene glycol monoricinoleate.

[0079] In this embodiment, the reaction product was detected by gas chromatography and the structure was correct. The conversion rate of the target product was determined to be 99.7%, and the selectivity of polyethylene glycol monoricinoleate was 95.5%.

[0080] Example 5

[0081] Take a three-necked flask equipped with a stirrer, a water separator and a condenser and connect a double-row tube for inert gas protection, add ricinoleic acid (1 mol), polyethylene glycol-1000 (1.5 mol), cyclohexane (300.0 g), hexaethyldisiloxane (1 wt% of the mass of ricinoleic acid) and methanesulfonic acid (0.1 wt% of the mass of ricinoleic acid) into the three-necked flask and mix thoroughly.

[0082] The stirring blade was turned on and the oil bath was controlled to heat, the reaction temperature was maintained at about 160°C, and the heating was continued for 10 hours. After the reaction, the heating was stopped when water was separated from the water separator. The collected reaction solution was subjected to reduced pressure distillation at 140°C and a vacuum degree of 10 KPa to remove the azeotrope of cyclohexane and water, and polyethylene glycol monoricinoleate was obtained.

[0083] In this embodiment, the reaction product was detected by gas chromatography and the structure was correct. The conversion rate of the target product was determined to be 82.1%, and the selectivity of polyethylene glycol monoricinoleate was 91.6%.

[0084] Example 6

[0085] Take a three-necked flask equipped with a stirrer, a water separator and a condenser and connect a double-row tube for inert gas protection, add ricinoleic acid (1 mol), polyethylene glycol-2000 (1.3 mol), xylene (300.0 g), tetradecamethylhexasiloxane (accounting for 20 wt% of the mass of ricinoleic acid) and acetic acid (accounting for 2.0 wt% of the mass of ricinoleic acid) into the three-necked flask and mix thoroughly.

[0086] Turn on the stirring blade and control the oil bath heating, keep the reaction temperature at about 200°C, and heat for 2 hours. After the reaction, stop heating when water is separated from the water separator. Perform reduced pressure distillation on the collected reaction solution at 140°C and a vacuum degree of 10KPa to remove the azeotrope of xylene and water to obtain polyethylene glycol monoricinoleate.

[0087] In this embodiment, the reaction product was detected by gas chromatography and the structure was correct. The conversion rate of the target product was determined to be 86.2%, and the selectivity of polyethylene glycol monoricinoleate was 87.2%.

[0088] Example 7

[0089] Take a three-necked flask equipped with a stirrer, a water separator and a condenser and connect a double-row tube for inert gas protection, add ricinoleic acid (1 mol), polyethylene glycol-5000 (1.1 mol), toluene (300.0 g), methyl octadecanoic acid (accounting for 8 wt% of the mass of ricinoleic acid) and p-toluenesulfonic acid (accounting for 1.0 wt% of the mass of ricinoleic acid) into the three-necked flask and mix thoroughly.

[0090] Turn on the stirring blade and control the oil bath heating, keep the reaction temperature at about 140°C, and heat for 10 hours. After the reaction, stop heating when water is separated from the water separator. Perform reduced pressure distillation on the collected reaction solution at 140°C and a vacuum degree of 10KPa to remove the azeotrope of toluene and water to obtain polyethylene glycol monoricinoleate.

[0091] In this embodiment, the reaction product was detected by gas chromatography and the structure was correct. The conversion rate of the target product was determined to be 88.9%, and the selectivity of polyethylene glycol monoricinoleate was 89.1%.

[0092] Comparative Example 1

[0093] The preparation method of polyethylene glycol monoricinoleate in this comparative example is the same as that in Example 1, except that the hexaphenyl disiloxane is not added. The reaction product is detected by gas chromatography, and the structure is correct. The conversion rate of the target product is determined to be 98.1%, and the selectivity of polyethylene glycol monoricinoleate is 82.1%.

[0094] Comparative Example 2

[0095] The preparation method of polyethylene glycol monoricinoleate in this comparative example is the same as that in Example 1, except that the water entrainer is not added. The reaction product is detected by gas chromatography, and the structure is correct. The conversion rate of the target product is 51.2%, and the selectivity of polyethylene glycol monoricinoleate is 92.6%.

[0096] Comparative Example 3

[0097] The preparation method of polyethylene glycol monoricinoleate in this comparative example is the same as that in Example 1, except that an equal amount of polymethylhydrogensiloxane is added to replace the hexaphenyldisiloxane. The reaction product is detected by gas chromatography and the structure is correct. The conversion rate of the target product is determined to be 98.7%, and the selectivity of polyethylene glycol monoricinoleate is 82.5%.

[0098] Comparative Example 4

[0099] The preparation method of polyethylene glycol monoricinoleate in this comparative example is the same as that in Example 1, except that an equal amount of hexachlorodisiloxane is added to replace the hexaphenyldisiloxane. The reaction product is detected by gas chromatography and the structure is correct. The conversion rate of the target product is determined to be 98.2%, and the selectivity of polyethylene glycol monoricinoleate is 81.7%.

[0100] Comparative Example 5

[0101] The preparation method of polyethylene glycol monoricinoleate in this comparative example is the same as that in Example 1, except that an equal amount of heptamethylcyclotetrasiloxane is added to replace the hexaphenyldisiloxane. The reaction product is detected by gas chromatography and the structure is correct. The conversion rate of the target product is determined to be 99.4%, and the selectivity of polyethylene glycol monoricinoleate is 95.3%.

[0102] Comparative Example 6

[0103] The preparation method of polyethylene glycol monoricinoleate in this comparative example is the same as that in Example 1, except that an equal amount of tert-butyl hydroquinone antioxidant is added to replace the hexaphenyl disiloxane. The reaction product is detected by gas chromatography and the structure is correct. The conversion rate of the target product is determined to be 98.6%, and the selectivity of polyethylene glycol monoricinoleate is 80.3%.

[0104] Experimental example

[0105] 1. Physical and chemical parameter test

[0106] The polyethylene glycol monoricinoleate prepared in the above Examples 1-7 and Comparative Examples 1-6 were respectively tested for physical and chemical indicators. The test indicators and test methods are as follows:

[0107] Color number test: APHA platinum-cobalt colorimetry method is used.

[0108] The physicochemical index results of the polyethylene glycol monoricinoleate products prepared in the above-mentioned embodiments and comparative examples are shown in Table 1 below.

[0109] Table 1 Physical and chemical index results of polyethylene glycol monoricinoleate

[0110] serial number Color Example 1 18Hazen Example 2 25Hazen Example 3 52Hazen Example 4 45Hazen Example 5 56Hazen Example 6 61Hazen Example 7 58Hazen Comparative Example 1 92Hazen Comparative Example 2 87Hazen Comparative Example 3 76Hazen Comparative Example 4 112Hazen Comparative Example 5 83Hazen Comparative Example 6 61Hazen

[0111] It can be seen that the preparation method of polyethylene glycol monoricinoleate described in the present application can obtain high-quality polyethylene glycol monoricinoleate with low color number under a catalytic system by adding siloxane as a modifier.

[0112] 2. Application performance

[0113] In this experimental example, polyethylene glycol monoricinoleate prepared in the above-mentioned Examples 1-7 and Comparative Examples 1-6 was used as a coating additive for painting and coating. The specific painting process and coating process methods refer to the method provided in the paper "Preparation and Performance Study of Water-Based Metallic Flash Coatings for Automobiles".

[0114] In this experimental example, the performance of the coating product prepared by using the above-mentioned polyethylene glycol monoricinoleate as a coating additive was measured respectively, and the test indicators and test methods were as follows:

[0115] Dynamic color index: SGY-A flash index measuring instrument, using the internationally common 15°, 45°, 110° three measuring angles for measurement. Calculation formula: FI = [2.69 (L* 15 -L* 110 ) 1.11 / (L* 45 ) 0.86 ].

[0116] The performance results of coating products prepared from the polyethylene glycol monoricinoleate products prepared in the above embodiments and comparative examples are shown in Table 2 below.

[0117] Table 2 Performance index results of coatings prepared by polyethylene glycol monoricinoleate

[0118] serial number Dynamic Color Index Example 1 26.3 Example 2 25.6 Example 3 24.8 Example 4 25.2 Example 5 24.2 Example 6 23.7 Example 7 24.1 Comparative Example 1 19.7 Comparative Example 2 21 Comparative Example 3 21.9 Comparative Example 4 18.8 Comparative Example 5 21.2 Comparative Example 6 21.6

[0119] It can be seen that the polyethylene glycol monoricinoleate described in the present application can be used as a coating additive to prepare high-quality polyethylene glycol monoricinoleate coating products with a high dynamic color index.

[0120] In summary, the preparation method of polyethylene glycol monoricinoleate of the present invention is based on the traditional esterification reaction system, and solves the problems of dark color and poor performance of the prior art products by adding a water entrainer and a modifier to the reaction system, especially as a coating additive to obtain a coating product with a high dynamic color index.

[0121] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing polyethylene glycol monoricinoleate, characterized in that: The method comprises the steps of using polyethylene glycol and ricinoleic acid as raw materials, adding a water co-boiling agent and a siloxane modifier to carry out esterification synthesis in the presence of an acid catalyst.

2. The method for preparing polyethylene glycol monoricinoleate according to claim 1, characterized in that: The siloxane modifier includes one or a mixture of hexamethyldisiloxane, octamethyltrisiloxane, hexaethyldisiloxane, hexaphenyldisiloxane, methyloctadecanoylsiloxane or tetradecamethylhexasiloxane; Preferably, the siloxane modifier comprises hexaphenyldisiloxane and / or hexamethyldisiloxane.

3. The method for preparing polyethylene glycol monoricinoleate according to claim 1 or 2, characterized in that: The amount of the silicone modifier added is 1-20wt% of the mass of the ricinoleic acid; Preferably, the added amount of the siloxane modifier is 5-10 wt % of the mass of the ricinoleic acid.

4. The method for preparing polyethylene glycol monoricinoleate according to any one of claims 1 to 3, characterized in that: The water entrainer includes an organic solvent that can form an azeotrope with water; Preferably, the water entrainer comprises one or a mixed solvent of n-hexane, cyclohexane, n-heptane, n-octane, toluene, benzene, xylene or n-decane; Preferably, the water entrainer comprises n-heptane and / or n-octane.

5. The method for preparing polyethylene glycol monoricinoleate according to any one of claims 1 to 4, characterized in that: The molar ratio of the polyethylene glycol to the ricinoleic acid is 1.0-1.5:

1.

6. The method for preparing polyethylene glycol monoricinoleate according to any one of claims 1 to 5, characterized in that: The polyethylene glycol includes one or a mixture of polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, polyethylene glycol-1000, polyethylene glycol-2000 or polyethylene glycol-5000; Preferably, the polyethylene glycol includes one of polyethylene glycol-400, polyethylene glycol-600 or polyethylene glycol-800 or a mixture of several thereof.

7. The method for preparing polyethylene glycol monoricinoleate according to any one of claims 1 to 6, characterized in that: The acidic catalyst includes at least one of an organic acid catalyst or an inorganic acid catalyst; Preferably, the acidic catalyst comprises one or a mixture of sulfuric acid, acetic acid, p-toluenesulfonic acid, methanesulfonic acid, benzoic acid or phenylacetic acid; Preferably, the acidic catalyst comprises methanesulfonic acid and / or p-toluenesulfonic acid; Preferably, the amount of the acidic catalyst is 0.1-2.0 wt % of the mass of the ricinoleic acid.

8. The method for preparing polyethylene glycol monoricinoleate according to any one of claims 1 to 7, characterized in that: The temperature of the esterification reaction is 100-200°C, preferably 120-160°C; and / or, The reaction time of the esterification reaction is 2-24h; Preferably, the method further comprises the steps of collecting the esterification reaction product and removing the azeotrope formed by the water entrainer and water.

9. Polyethylene glycol monoricinoleate prepared by the method according to any one of claims 1 to 8.

10. Use of the polyethylene glycol monoricinoleate according to claim 9 for preparing a high dynamic color index coating product.

Citation Information

Patent Citations

  • Method for synthesis of polyethylene glycol monoricinoleate by borate method

    CN102816324A

  • Method for preparing castor oil-based polysiloxane polyol

    CN101775141A

  • Method for preparing poly castor oleate

    CN102504234A

  • Preparation method of glycol ricinoleic acid monoester and use and coating of glycol ricinoleic acid monoester

    CN110437071A

  • Polyol fatty acid ester / phenyl / polyether co-modified silicone oil, preparation method and special low-silicon oil agent for carbon fibers

    CN112778527A