Preparation and application of rosin-based tri-crosslinked polyamide
Through the acid chloride condensation method and the Yamazaki-Higashi polycondensation method, fumazaki acid and diamine were reacted to prepare a rosin-based tri-crosslinked polyamide, which solved the problems of low molecular weight and poor crystallinity of the rosin derivative polyamide, and achieved high Stability and acid-base-resistant polymers have expanded the application potential of polyamides.
Patent Information
- Application Number
- CN202411266684.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, rosin derivatives are used to prepare polyamides with low molecular weight and poor crystallinity, and there are few researches on ternary crosslinked polyamides, especially the polymerization of fumashiro acid acid chloride and diamine compounds to form ternary crosslinks. There are no reports of polyamides, and the traditional polymerization reaction conditions are harsh, making it difficult to form a crosslinked polymer that is resistant to high temperature and acid and alkali.
The acid chloride condensation method and the Yamazaki-Higashi polycondensation method were used to react fumazaki acid with diamine to prepare a rosin-based tri-crosslinked polyamide, which was polymerized at room temperature by acid chloride condensation method. The reaction conditions were mild and the time was short; Yamazaki-Higashi polycondensation method is used for the synthesis of aromatic polyamides, expanding to the direct condensation of tricarboxylic acid and diamine to form a tri-crosslinked rosin-based crosslinked polyamide.
The prepared rosin-based tri-crosslinked polyamide has good stability, high strength, high temperature resistance, and excellent acid and alkali corrosion resistance. It is suitable for structural materials, high temperature resistance and acid and alkali corrosion resistance and is suitable for the fields of structural materials, high temperature resistance and acid and alkali corrosion resistance, making up for the rosin-based poly Vaccine in amide-related synthesis.
Smart Images

Figure CN118930846A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer chemistry, and specifically to preparing rosin-based cross-linked polyamide by condensing rosin-derived downstream products with acyl chloride or Yamazaki-Higashi polycondensation, belonging to the field of polymer material preparation and application. Background Art
[0002] Polyamide, also known as Polyamide (PA), is a general term for polymers containing amide groups in the repeating units of the main chain of macromolecules. The main chain of polyamide contains a large number of polar amide groups. Amide groups have elements such as N and O that are easy to form hydrogen bonds with H-bond donors. They can form hydrogen bonds with phenols, quinones, nitro compounds, etc. and be adsorbed, and then separated from compounds that cannot form hydrogen bonds; therefore, using polyamide as a chromatography column filler can separate and purify certain substances within a certain polarity range. There is a strong interaction between polyamide molecules. Their excellent performance in mechanical strength, flexibility, toughness and tolerance makes polyamide materials used in many fields such as automobiles and aircraft, fibers, electrical appliances and engineering, and medical treatment. In addition to petroleum-based polyamides, many bio-based polyamides have also been developed recently, with important structures and properties.
[0003] Rosin is a renewable natural chemical raw material, a mixture of various resin acids, fatty acids and neutral substances. Resin acid is the main component of rosin and is also a general term for a class of compounds. The common feature of its structure is the presence of a monobasic acid with a phenanthrene ring skeleton and two double bonds. Rosin and its derivatives are widely used in adhesives, coatings, inks and other industries with their unique properties. In recent years, with the shortage of petroleum resources, researchers from all over the world have begun to explore renewable resources that can replace petroleum to produce polymer materials. With its unique composition and structure, rosin has begun to be used as a polymer monomer in the synthesis of various polymer materials. Rosin contains about 90% of resin acids, about 10% of esters and unsaponifiable substances. The main component of resin acid is abietic acid with conjugated double bonds. The conjugated double bonds in the molecular structure of abietic acid are not in the same alicyclic ring, so it cannot undergo Diels-Alder reaction with dienophiles such as fumaric acid, but abietic acid can be converted into pimaric acid through isomerization reaction at high temperature. Pimaric acid can be reacted with a dienophile such as fumaric acid to obtain rosin derivatives such as fumaric acid by Diels-Alder reaction. Xu et al. reacted fumaric acid with thionyl chloride to obtain fumaric acid chloride, which was then reacted with ammonia to synthesize fumaric acid amide, which is a small molecule compound. Roy et al. (Eur Polym J, 1990, 26 (4): 471-474.) used rosin diacid (APA), a DA addition product of rosin and acrylic acid, to perform chlorination, and then reacted with hexamethylenediamine to synthesize rosin-based polyamide, but the results showed that the polyamide had a low molecular weight and poor crystallinity. Bicu I et al. prepared polyamide using rosin derivative dibasic acid propylene pimaric acid ketone (DAPK) and polyamines such as triethylenetetramine (Polym Sci Part A: Polym Chem, 2007, 45 (24): 5979-5990) and ethylenediamine (Polym Sci Part A: Polym Chem, 2005, 43 (24): 6308-6322), but the molecular weight of the synthesized polyamide is not high. At present, there are relatively few studies on ternary cross-linked polyamide and rosin-based polyamide, and there is no report on the polymerization of fumaric pimaric acid chloride and diamine compounds to form ternary cross-linked polyamide.
[0004] Polyamide is generally polymerized from diacid and diamine, but due to its harsh reaction conditions, it is usually reacted under high temperature and high pressure. Zhou Yang et al. (Polymer Materials Science and Engineering, 2024, 40(02): 9-19.) used dicarboxylic acid and diamine to form a nylon salt intermediate, washed and then heated to a molten state for polycondensation. This method requires the formation of a nylon salt monomer and a high-temperature reaction, which is time-consuming and labor-intensive, and the conditions are relatively harsh. Kurose Hideyuki et al. disclosed a method for direct melt polymerization of a dicarboxylic acid component and a diamine component in the absence of a solvent. By heating the diacid component to a temperature higher than the melting point of the produced polyamide, the diamine component is added while the reactant diacid component is kept in a molten state. This method reduces the synthesis steps of the nylon salt intermediate, but it still reacts in a high-temperature molten state, and the reaction conditions are also relatively harsh. Cao Yu et al. (Chemistry and Bioengineering, 2007, (05): 60-63) et al. prepared a gray powder small molecule polyamide by reacting maleic rosin chloride with ethylenediamine at 40°C for 2h. However, the two amide groups of the maleic rosin chain in the polymer are in the cis position, and it is easy to cyclize into a structure of intracyclic diimide under slightly higher temperature conditions, which makes it difficult to form a cross-linked polyamide polymer material. In addition, the stability of such polymers is poor and there is no potential for practical application. The present invention is to obtain a rosin-based three-crosslinked polyamide by polymerizing fumaric pimaric acid chloride with diamine, which has no cyclizable cis diacyl structure and is easy to form a high temperature resistant, acid and alkali corrosion resistant, high strength rosin-based crosslinked polymer. The prepared polymer has great application potential in structural materials, high temperature resistant materials, corrosion resistant materials, etc. The acyl chloride condensation method of the present invention can usually polymerize at room temperature, with mild reaction conditions and short reaction time; the Yamazaki-Higashi polycondensation method is generally used for the synthesis of wholly aromatic polyamides and for the polymerization of aromatic diacids and aromatic diamines. Wang Zhao et al. reported on the synthesis of dibenzo-octacyclic polyarylamide by the Yamazaki-Higashi polycondensation method at the 2017 National Polymer Academic Paper Conference of the Chinese Chemical Society. This paper uses the Yamazaki-Higashi polycondensation method to directly condense fumaric acid tricarboxylic acid with diamine to obtain a three-crosslinked rosin-based crosslinked polyamide, which expands the application of the Yamazaki-Higashi polycondensation method in the polymerization of tricarboxylic acids. Summary of the invention
[0005] The present invention utilizes the existing technology to develop a rosin-based three-crosslinked polyamide polymer material, and provides two methods for synthesizing the rosin-based three-crosslinked polyamide by using fumaric acid, a downstream product of rosin, as a raw material. The rosin-based three-crosslinked polyamide has the characteristics of good stability, high strength, high temperature resistance, acid and alkali resistance, etc., and can be used in various structural materials, high temperature resistant materials, acid and alkali corrosion resistant materials and other fields after being treated or modified.
[0006] The present invention has six invention contents: Summary of the invention 1:
[0008] The present invention is a rosin-based three-crosslinked polyamide polymer, and its structural formula is shown in Formula 1 in Claim 1. Taking the polymer of ethylenediamine in the diamine monomer as an example, its common name is polyfumaric acid triethylenediamine, and its semi-systematic chemical name is poly-8,12-ethyl-bridged rosin-13-ene-4,21,22-triformyl triethylenediamine, and it has a structure of Formula 4:
[0009] The physical and chemical properties of polyfumaric acid triethylenediamine: white solid in appearance, insoluble in organic solvents such as methanol, anhydrous ethanol, gasoline, cyclohexane, toluene, acetone, acetic acid, dichloromethane, N, N-dimethylformamide, etc., decomposition temperature is 350℃, melting point is 340℃. Summary of the invention 2:
[0011] The rosin-based three-crosslinked polyamide polymer is prepared by the acyl chloride condensation method. The granular polymer can be obtained by solution polymerization, or the polyamide film can be obtained by interfacial polymerization. The tricarboxylic acid fumaric acid synthesized from rosin is chlorinated and then reacted with a diamine compound to form a three-crosslinked polyamide.
[0012] As a preferred technical solution, the preparation method of fumaric acid pimaric acid chloride in the acyl chloride condensation method comprises the following steps:
[0013] Step 1: After the purified fumaric acid is confirmed to have no impurities by TLC plate, fumaric acid, 4-dimethylaminopyridine and dithionyl chloride are added into a three-necked flask in sequence, and the reaction temperature is 60°C. The reaction time is 6 hours. The molar ratio of fumaric acid to dithionyl chloride is 1:15, and the amount of 4-dimethylaminopyridine is about 5% of the mass of fumaric acid.
[0014] Step 2: Connect the three-necked flask in step 1 to anhydrous calcium chloride for drying, and finally connect it to sodium hydroxide solution to absorb the volatilized thionyl chloride. Use a rotary evaporator to remove the unreacted thionyl chloride from the product after the reaction. Vacuum the product, and start filling it with nitrogen after vacuuming to prevent the acid chloride from hydrolyzing back to carboxylic acid.
[0015] As a preferred technical solution, the synthesis of rosin-based cross-linked polyamide by acyl chloride polycondensation method includes the following steps:
[0016] Step 1: Prepare the oil phase. The acyl chloride is ultrasonically dissolved in an organic solvent at a concentration of 0.24 mol / L
[0017] Step 2: Prepare the aqueous phase, add alkali into water and stir to dissolve, the concentration is 0.86moL / L.
[0018] Step 3: Pour the acyl chloride solution into a three-necked flask, start stirring, slowly add the diamine during stirring to make it fully mixed, then slowly pour the alkali aqueous solution and react for 0.5h. Then filter to obtain a solid polymer, extract the filtered product with anhydrous ethanol for 24 hours to remove unreacted raw materials and other impurities, and dry it in an oven to obtain a white or brown, granular or blocky rosin-based cross-linked polyamide solid.
[0019] Step 4: Soak the base film in a mixed aqueous solution of alkali and diamine for 3 minutes and then take it out. After there is no obvious liquid on the surface of the membrane, soak it in an acyl chloride solution for 3 minutes, wash away the unreacted raw materials with xylene, and put it in an oven for drying to obtain a white or light yellow flaky rosin-based cross-linked polyamide composite membrane.
[0020] In the present invention, the diamine described in the preparation process is any one of C2-C6 diamine compounds such as ethylenediamine and hexamethylenediamine, or aromatic diamine compounds such as p-phenylenediamine.
[0021] In the present invention, the base in the preparation process is any one of potassium hydroxide, sodium hydroxide and triethylamine. Summary of the invention 3:
[0023] Preparation of rosin-based three-crosslinked polyamide polymer, as a preferred technical solution, the synthesis of rosin-based crosslinked polyamide by Yamazaki-Higashi polycondensation method includes the following steps.
[0024] Step 1: Since lithium chloride easily absorbs moisture and becomes damp, it needs to be placed in a vacuum drying oven for vacuum drying before the reaction to remove moisture and prevent moisture from hindering the condensation of acid amine.
[0025] Step 2: Add fumaric acid, diamine compound and lithium chloride to the reaction bottle in sequence, evacuate, fill with nitrogen for protection, and add pyridine, triphenyl phosphite and N-methylpyrrolidone in sequence under nitrogen atmosphere. Gradually heat to 100°C under nitrogen conditions and react for 6 hours. After the reaction, add methanol to precipitate the crude product. Soak and rinse the crude product with water, methanol and ethanol respectively, filter and vacuum dry to obtain the polyamide product.
[0026] In the present invention, the diamine compound in step 2 is an aromatic diamine compound such as p-phenylenediamine, and the molar ratio of fumaric acid to diamine is 1:1.8.
[0027] In the present invention, the molar ratio of fumaric acid chloride to diamine is 1:1.65.
[0028] In the present invention, the organic solvent is any one of xylene, toluene, dichloromethane and tetrahydrofuran.
[0029] In the present invention, the alkali solution is one of potassium hydroxide, sodium hydroxide and triethylamine, and the amount of the alkali used is 2.2 times the amount of the diamine.
[0030] The present invention has the following advantages
[0031] 1. The raw materials are downstream products of natural products, which are easy to obtain, and enrich the method of using fumaric acid, a downstream product of rosin, as a raw material to prepare polyamide.
[0032] 2. The Yamazaki-Higashi polycondensation method was used to prepare a rosin-based cross-linked polyamide with a cross-linked trimer structure of fumaric acid and diamine, which expanded the application of the Yamazaki-Higashi polycondensation method in the polymerization of tricarboxylic acids.
[0033] 3. The product is rosin-based polyamide, which has strong solvent resistance and high temperature resistance.
[0034] 4. The raw materials are extensive and the product performance is good. This method fills the gap in the synthesis of rosin-based polyamide. Summary of the invention 4:
[0036] The prepared rosin-based three-crosslinked polyamide polymer has good acid and alkali corrosion resistance. The specific acid and alkali corrosion resistance test includes the following steps:
[0037] Step 1: prepare an acid or base of a certain concentration, and then soak a certain amount of rosin-based three-crosslinked polyamide polymer in the acid for 4h-24h.
[0038] Step 2: Acid corrosion test After soaking in acid solution for a set time, quench the acid with saturated sodium bicarbonate solution and filter, rinse with water, methanol, and anhydrous ethanol to remove the generated salt and the decomposition products of polyamide. Put the remaining solid into the oven to dry, weigh and record the mass.
[0039] Step 3: Alkali corrosion test After soaking in alkaline solution for a set time, neutralize the alkaline solution with 10% hydrochloric acid solution until it is neutral, then filter it, rinse it with water, methanol, and anhydrous ethanol to remove the generated salt and the decomposition products of polyamide. Put the remaining solid into the oven to dry, weigh and record the mass.
[0040] In the present invention, the acid concentration used in step 2 is any one of 36.5% concentrated hydrochloric acid, 98% formic acid, and 40% concentrated hydrochloric acid. The base used in step 3 is any one of 40% sodium hydroxide, potassium hydroxide, and 1,5-diazabicyclo[4.3.0]-5-nonene (DBN). Summary of the invention 5:
[0042] The prepared rosin-based three-crosslinked polyamide polymer has good thermal stability. According to the definition of thermal stability of a substance in the national standard GB / T13464-2008 Thermal Analysis Test Method for Thermal Stability of a Material, a substance is considered stable if it does not undergo enthalpy change under certain conditions. Thermal stability is tested by differential scanning calorimetry (DSC) and its spectrum is analyzed. The thermal stability of the rosin-based three-crosslinked polyamide polymer is shown in the DSC test results (see Appendix Figure 3 ), the enthalpy of evaporation of water is around 100°C, and there is no other enthalpy change before 330°C. According to the definition of national standards, the polymer is stable within this temperature range. Therefore, the rosin-based three-crosslinked polyamide polymer has good thermal stability before 330°C. Description of the accompanying drawings
[0043] Figure 1 This is the infrared spectrum of fumaric acid chloride
[0044] Figure 2 This is the infrared spectrum of rosin-based cross-linked polyamide
[0045] Figure 3 This is the DSC curve of rosin-based cross-linked polyamide
[0046] Figure 4 This is the TG curve of rosin-based cross-linked amide
[0047] Note: Figure 2 , 3 The English abbreviations in 4 correspond to the substances poly(triethylene fumarate) (PA2FP), poly(trihexyl fumarate) (PA6FP), poly(tri-p-phenylenediamine fumarate) (PADAFP), poly(tridecyl fumarate) (PA10FP), poly(tridodecyl fumarate) (PΛ12FP) DETAILED DESCRIPTION
[0048] The present invention is further explained with reference to the following examples, but the present invention is not limited to the following examples.
[0049] The reaction principles and catalysts used in the embodiments of the present invention are all conventional commercially available reagents on the market unless otherwise specified.
[0050] The intermediate product of fumaric acid chloride of the present invention adopts a unified experiment and treatment method, and better experimental conditions are yet to be explored.
[0051] The rosin-based tribasic acid used, namely fumaric acid, is a self-made product. Fumaric acid is synthesized by Diels-Alder addition reaction with rosin and fumaric acid as raw materials. The Diels-Alder addition reaction conditions are: weigh a certain amount of rosin and fumaric acid (the fumaric acid is 30% of the mass of the rosin), the reaction time is 3 hours, the reaction temperature is 210°C, the obtained crude product is purified by potassium salting, multiple recrystallization and other steps, and finally converted into pure fumaric acid by acidification. The specific preparation can refer to the literature: "Preparation method of fumaric acid" patent, application number: CN200910033428.5
[0052] Example 1
[0053] (I) Synthesis of Fumaropimaric Acid Chloride
[0054] In a 1000mL three-necked flask equipped with a heating jacket, a magnet, and a thermometer, add 24g of fumaric acid and 80g of rosin in turn, evacuate the three-necked flask for 5-10min, and insert a nitrogen bag. Heat to 210℃, start stirring after the solid is completely dissolved, and the reaction time is 3h. After the reaction is completed, cool the three-necked flask to room temperature and add 400mL of anhydrous ethanol, stirring and dissolving at 80℃. While the solid is dissolving, heat and dissolve 15g of potassium hydroxide with 150mL of ethanol. After the solid is completely dissolved, add the hot potassium hydroxide ethanol solution to the three-necked flask and react for 30min. After the reaction is completed, pour it into a Buchner funnel and filter it, then dry it in an oven. After drying, heat and dissolve with 50% ethanol solution (i.e., water and anhydrous ethanol 1:1), then cool to room temperature and put into a refrigerator for cooling and crystallization for 7-8 hours, then take out the crystallized solid and filter it with ethanol, then put it into an oven for drying, repeat the above recrystallization operation 2-3 times to obtain pure potassium fumaric acid. Potassium fumaric acid is dissolved with 60% ethanol solution to a particle-free state, then 8% hydrochloric acid aqueous solution is added while stirring until the solution pH is about 1, then distilled water is poured into it while stirring until no white matter is precipitated, and pure fumaric acid is obtained.
[0055] After drying the fumaric acid, confirming that there is no rosin and fumaric acid impurities through the TCL plate, 5g of fumaric acid and 0.22g of 4-dimethylaminopyridine are added to a 250mL three-necked flask in turn, and 15mL of dichlorothionyl is slowly added dropwise while stirring. The reaction temperature is 70°C and the reaction time is 8h. After the reaction is completed, a small amount of the reaction solution is taken, diluted with methanol, and the ester is generated by the acyl chloride and methanol. The TCL plate is used to monitor whether the fumaric acid is fully reacted. Most of the unreacted dichlorothionyl is removed by a water pump and a Montessori washing bottle, and a small amount of dichloromethane is added to remove dichloromethane and dichlorothionyl on a rotary evaporator. The fumaric acid chloride after the rotation is evacuated and filled with nitrogen for protection and storage.
[0056] Example 2
[0057] Synthesis of poly(trihexylene fumarate)pimaracamide
[0058] 2.088g of fumaric acid chloride and 57mL of xylene were added to a 250mL three-necked flask to dissolve, and 0.9162g of hexamethylenediamine was added and stirred for 10 minutes during stirring. The aqueous phase was prepared while stirring, and 57mL of water and 0.55g of potassium hydroxide were added to a 100mL beaker. Then, the aqueous phase was poured into the three-necked flask during stirring, and the aqueous phase was stirred for 5 minutes after the aqueous phase was added, and then filtered to obtain a polyamide solid. The solid was soaked in a Soxhlet extractor for two days to obtain 1.622g of brown polyfumaric acid trihexamethylenediamine solid with a melting point of 340°C.
[0059] Example 3
[0060] Synthesis of poly(tri-p-phenylenediamine)-pimaracamide
[0061] The synthesis method is basically the same as that of Example 2, except that the xylene in Example 2 is replaced by tetrahydrofuran, hexamethylenediamine is replaced by p-phenylenediamine, and 0.55g potassium hydroxide in the aqueous phase is replaced by 2.41mL triethylamine. 20mL tetrahydrofuran is taken to dissolve 2.088g fumaric acid chloride and 0.8526g p-phenylenediamine, and the chloride solution is first poured into a three-necked flask, and then the p-phenylenediamine solution is poured into the stirring process. Finally, 1.561g polyfumaric acid tri-p-phenylenediamine brown solid is obtained, with a melting point of 350°C.
[0062] Example 4
[0063] Synthesis of Poly(Fumaracanoyl Tridecyldiamine)
[0064] The synthesis method is basically the same as that of Example 2, except that the xylene in Example 2 is replaced by dichloromethane, hexamethylenediamine is replaced by decanediamine, and 0.55g potassium hydroxide in the aqueous phase is replaced by 2.41mL triethylamine. Take 20mL of dichloromethane to dissolve 2.088g of fumaric acid chloride and 1.3585g of decanediamine, respectively, first pour the acid chloride solution into a three-necked flask, and then pour the decanediamine solution into the stirring process. Finally, 1.837g of polyfumaric acid tridecane diamine white solid is obtained, with a melting point of 340°C.
[0065] Example 5
[0066] Synthesis of poly(triethylenediamine)fumarate
[0067] The synthesis method is basically the same as that of Example 2, except that the xylene in Example 2 is replaced by tetrahydrofuran, hexamethylenediamine is replaced by ethylenediamine, and 0.55g potassium hydroxide in the aqueous phase is replaced by 2.41mL triethylamine. 0.53mL ethylenediamine is slowly added dropwise during stirring. Finally, 1.336g polyfumaric acid triethylenediamine white solid is obtained, with a melting point of 340°C.
[0068] Example 6
[0069] Synthesis of poly(fumaric acid tridodecylene diamine)
[0070] The synthesis method is basically the same as that of Example 2, except that: the hexamethylenediamine in Example 2 is replaced with 1,12-diaminododecane, the solvent of the aqueous phase is changed to xylene, and 0.55g potassium hydroxide is changed to 2.41mL triethylamine. Take 20mL xylene to dissolve 2.088g fumaric acid chloride and 1.5796g 1,12-diaminododecane, first pour the 1,12-diaminododecane solution into a three-necked flask, and then pour the acid chloride solution into the stirring process. Finally, 1.933g polyfumaric acid tridodecyl diamine brown solid is obtained, with a melting point of 345°C.
[0071] Example 7
[0072] Preparation of poly(trihexylene fumarate) film by interfacial polymerization
[0073] Take a 100mL small beaker and a 250mL beaker, dissolve 2.088g of fumaric acid chloride in 57mL of dichloromethane in the 250mL beaker, and dissolve 0.9162g of hexamethylenediamine and 0.55g of potassium hydroxide in 57mL of water in the 100mL beaker. Then extend a glass rod to the bottom of the 250mL beaker, and slowly pour the hexamethylenediamine aqueous phase into the chloride solution along the glass rod. A light yellow vein film appears between the two phases in the beaker.
[0074] Example 8
[0075] Preparation of poly(triethylenediamine fumarate) film by interfacial polymerization
[0076] Take a 100mL small beaker and a 250mL beaker, dissolve 2.088g of fumaric acid chloride in 57mL of dichloromethane in the 250mL beaker, and dissolve 0.53mL of ethylenediamine and 0.55g of potassium hydroxide in 57mL of water in the 100mL beaker. Then extend a glass rod to the bottom of the 250mL beaker, and slowly pour the ethylenediamine aqueous solution into the acid chloride solution along the glass rod. A thin film appears between the two phases in the beaker.
[0077] Example 9
[0078] Preparation of poly(fumaric acid trihexylene diamine) composite membrane
[0079] Take a 100mL small beaker and a 250mL beaker, dissolve 2.088g of fumaric acid chloride in 57mL of xylene in the 250mL beaker, and dissolve 0.9162g of hexamethylenediamine and 0.55g of potassium hydroxide in 57mL of water in the 100mL beaker. Then soak the polyethersulfone membrane in the water phase for 3min, take it out and dry it, soak it in the chloride solution for 3min, and put it in an oven to dry. After drying, there is a light yellow polyfumaric acid trihexamethylenediamine coating layer on the polyethersulfone membrane.
[0080] Example 10
[0081] Preparation of poly(fumaric acid triethylenediamine) composite membrane
[0082] Take a 100mL small beaker and a 250mL beaker, dissolve 2.088g of fumaric acid chloride in 57mL of xylene in the 250mL beaker, and dissolve 0.53mL of ethylenediamine and 0.55g of potassium hydroxide in 57mL of water in the 100mL beaker. Then soak the polyethersulfone membrane in the water phase for 3min, take it out and dry it, soak it in the chloride solution for 3min, and put it in an oven to dry. After drying, there is a white polyfumaric acid triethylenediamine coating layer on the polyethersulfone membrane.
[0083] Embodiment 11
[0084] Condensation of Poly(pimaric acid-fumaric acid terephthalamide) by Yamszski-Higashi method
[0085] Take a 10mL micro reaction tube, add 0.2g of fumaric acid, 0.093g of p-phenylenediamine and 0.0488g of lithium chloride, evacuate and fill with nitrogen, add 0.6mL of pyridine, 0.2mL of triphenyl phosphite and 1.2mL of N-methylpyrrolidone in sequence under nitrogen conditions, and react for 8h after heating to 100℃. After the reaction is completed, rinse with methanol to precipitate white material. After rinsing with water, ethanol and methanol respectively, filter and vacuum dry the residue to obtain 0.161g of white polyfumaric acid terephthalamide solid.
[0086] Example 12
[0087] Yamazaki-Higashi Condensation of Poly(pimaric acid-fumaric acid terephthalamide)
[0088] Take a 10mL micro reaction tube, add 0.2g of fumaric acid, 0.1163g of p-phenylenediamine and 0.0488g of lithium chloride, evacuate and fill with nitrogen, add 0.6mL of pyridine, 0.2mL of triphenyl phosphite and 1.2mL of N-methylpyrrolidone in sequence under nitrogen conditions, and react for 8h after heating to 100℃. After the reaction is completed, rinse with methanol to precipitate white material. After rinsing with water, ethanol and methanol respectively, filter and vacuum dry the residue to obtain 0.149g of white polyfumaric acid pimaric acid terephthalamide solid.
[0089] Example 13
[0090] Test on the acid corrosion resistance of polypimaric acid terephthalamide
[0091] Take four 100mL round-bottom flasks, mark them as 1, 2, 3, and 4, then add 5mL of 36.5% concentrated hydrochloric acid into the round-bottom flasks, weigh 0.2g of polyfumaric acid terephthalamide into the round-bottom flasks and soak for 4h, 8h, 12h, and 24h respectively. Then quench the acid with saturated sodium bicarbonate solution and filter, rinse with water, methanol, and anhydrous ethanol respectively to remove the generated salt and the decomposition products of polyamide. Put the remaining solid into the oven to dry, weigh and record the mass. The final result shows that the residual mass percentage is above 91%.
[0092] Embodiment 14
[0093] Alkali corrosion resistance test of polypimaric acid terephthalamide
[0094] Take four 100mL round-bottom flasks, mark them as 1, 2, 3, and 4, then add 5mL of 40% potassium hydroxide solution into the round-bottom flasks, weigh 0.2g of polypimaric acid terephthalamide into the round-bottom flasks and soak for 4h, 8h, 12h, and 24h respectively. Then, quench the acid with saturated sodium bicarbonate solution and filter, rinse with water, methanol, and anhydrous ethanol respectively to remove the generated salt and the decomposition products of polyamide. The remaining solid was placed in an oven for drying, and the weight was recorded. The final result showed that the residual weight percentage was above 90%.
[0095] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. The rosin-based three-crosslinked polyamide of the present invention has the following structural characteristics: the rosin-based three-crosslinked polyamide chain segments contain triacyl groups and hydrocarbon diamino groups of the fumaric rosin-based phenanthrene ring. The rosin-based three-crosslinked polyamide has the structure described in Formula 1:
2. The rosin-based tri-crosslinked polyamide according to claim 1 can be prepared by condensing a rosin-derived carboxylic acid or an acid chloride, wherein: First, the acyl chloride condensation method, in which fumaric acid and dithionyl chloride react under the catalysis of 4-dimethylaminopyridine to obtain fumaric acid trichloride, and the fumaric acid trichloride and diamine undergo condensation polymerization to obtain a tri-crosslinked polyamide; Second, the Yamazaki-Higashi polycondensation method, in which fumaric acid and diamine undergo direct Yamazaki-Higashi polycondensation under the conditions of pyridine and N-methylpyrrolidone as solvents, lithium chloride and triphenyl phosphite as catalysts to obtain a rosin-based tri-crosslinked polyamide.
3. The rosin-based tri-crosslinked polyamide according to claim 1, characterized in that: Fumaropimaric acid, one of the raw materials, is a reaction product of diene synthesis of rosin and fumaric acid. The compound fumaropimaric acid has a structure shown in Formula 2. The intermediate product of the acyl chloride condensation method, fumaropimaric acid chloride, is obtained by acyl chloride of fumaropimaric acid and has a structure shown in Formula 3:
4. The rosin-based tri-crosslinked polyamide according to claim 1, wherein the precursor compound used in the acid chloride condensation method is fumaric acid trichloride, characterized in that The synthesis includes the following steps: Add the purified fumaric acid, 4-dimethylaminopyridine and thionyl chloride into a three-necked flask, connect the three-necked flask with anhydrous calcium chloride for drying, and finally connect the flask with sodium hydroxide solution to absorb the volatilized thionyl chloride. The reaction temperature is 60°C-80°C, preferably 70°C-80°C. The reaction time is 6h-10h, preferably 6h-8h. The product after the reaction is removed from the unreacted thionyl chloride using a rotary evaporator to obtain a brown solid. Finally, the product is evacuated into a vacuum and nitrogen is filled in to prevent the acid chloride from hydrolyzing back to carboxylic acid.
5. The rosin-based tri-crosslinked polyamide according to claim 1, when prepared by an acyl chloride condensation method, is characterized in that: The preparation process includes the following steps: (1) Prepare the oil phase Take fumaric acid chloride and dissolve it in an organic solvent such as toluene, dichloromethane, toluene, tetrahydrofuran, etc. by ultrasonication. (2) Preparation of water phase Add one of the bases such as potassium hydroxide, sodium hydroxide, triethylamine, etc. into water and stir to dissolve. (3) Polymerization reaction Pour the oil phase solution in which fumaric acid chloride is dissolved into a three-necked flask, start stirring, and slowly add diamine during stirring to fully mix. At the same time, slowly pour the aqueous alkali solution into the three-necked flask and stir it fully. (4) Impurity treatment The product of the previous step is filtered to remove the liquid and impurities dissolved in the liquid to obtain a crude polyamide product. The crude polyamide product is subjected to Soxhlet extraction with anhydrous ethanol to remove unreacted raw materials to obtain a pure rosin-based three-crosslinked polyamide solid.
6. The rosin-based tri-crosslinked polyamide according to claim 1, when synthesized by the Yamazaki-Higashi polycondensation method, is characterized in that: The following steps are involved: (1) Catalyst pretreatment Since lithium chloride easily absorbs moisture and becomes damp, it needs to be placed in a vacuum drying oven for vacuum drying before the reaction to remove moisture and prevent moisture from hindering the condensation of the acid amine. (2) Add fumaric acid, diamine compound and lithium chloride to the reaction bottle in sequence, evacuate the bottle, fill it with nitrogen for protection, and add pyridine, triphenyl phosphite and N-methylpyrrolidone in sequence under nitrogen atmosphere. Gradually increase the temperature to 100°C under nitrogen conditions and react for 6-8 hours. After the reaction is completed, add methanol to precipitate a crude product. (3) Product purification The crude product was soaked and washed with water, methanol and ethanol respectively, filtered and vacuum dried to obtain a rosin-based three-crosslinked polyamide product.
7. The rosin-based tri-crosslinked polyamide according to claim 1, characterized in that: The diamine used in the preparation is ethylenediamine, hexamethylenediamine, decanediamine, 1,12-dodecanediamine and the like C2-C 12 Any one of the diamine compounds, or aromatic diamine compounds such as p-phenylenediamine.
8. The rosin-based tri-crosslinked polyamide according to claim 1, when prepared by the acyl chloride condensation method in 2, the method for synthesizing the polyamide in 5 is characterized in that: The organic solvent is any one of xylene, toluene, dichloromethane and tetrahydrofuran.
9. The method of synthesizing polyamide by the Yamazaki-Higashi polycondensation method according to claim 6, characterized in that: The diamine is an aromatic diamine compound such as p-phenylenediamine.
Citation Information
Patent Citations
Rosin-based semi-alicyclic polyamide-imide PA6I and synthesizing method thereof
CN102718969A
Rosin-based self-repairing polymer, synthesis method and application thereof
CN112979908A
Saline-alkali tolerant super absorbent resin and preparation method thereof
CN113896843A
No title available
GB1232058A
Resins from maleopimaric acid and primary amines
US3637638A