Organic polymer electrode material and preparation method and application thereof
By designing organic polymer electrode materials containing pyrazine structure, using conjugated carbonyl linking groups, the problems of low capacity and poor conductivity of the positive electrode materials of lithium-ion batteries are solved, and high specific capacity and good cycle performance are achieved. It is suitable for use in Continuous, high energy density energy storage battery.
Patent Information
- Application Number
- CN202411138286.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The theoretical specific capacity of the existing lithium-ion battery positive electrode materials is relatively low, and the transition metal elements contain high costs, scarce resources, toxic and harmful. The organic electrode materials are easy to dissolve and have poor electrical conductivity, which limits their application.
Using organic polymer electrode materials containing tripyrazine structural units, using conjugated carbonyl as a linking group to design organic positive electrode materials with high conductivity and good rate performance, using tribromide tripyrazine monomer and diamino-containing group The polymerization reaction was carried out with the monomer of conjugated carbonyl group to prepare an organic conjugated polymer rich in C=N and C=O groups.
Achieve high theoretical specific capacity greater than 300mAh·g-1, good rate performance and cycle performance, solve the problems of low capacity, easy dissolution and poor conductivity of the positive electrode material of existing lithium-ion batteries, and provide low cost, environmental protection and sustainable energy storage battery material.
Smart Images

Figure CN118930853A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and specifically relates to an organic polymer electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion battery is a high-energy secondary battery with advantages such as high energy density, high operating voltage, long cycle life and wide operating temperature range. It is widely used in portable electronic devices, electric vehicles, smart grids and other fields. As one of the important components of lithium-ion batteries, positive electrode materials play a decisive role in the energy density and cost of lithium-ion batteries. At present, commercial lithium-ion battery positive electrode materials are mainly traditional lithium transition metal oxides and phosphates, such as LiCoO2, LiMn2O4, LiFePO4, etc. However, compared with the graphite negative electrode (theoretical specific capacity of 372mAh g -1 ), the theoretical specific capacity of these cathode materials is usually lower than that of conventional cathode materials, which has been considered the main bottleneck for the further development of lithium-ion batteries. In addition, these traditional inorganic cathode materials containing transition metal elements (Co, Ni, Mn, etc.) are generally expensive, scarce, toxic and harmful, poorly recyclable, and unfriendly to the environment. In the long run, humans may face a certain resource crisis. Therefore, in order to alleviate the increasingly severe energy depletion problem and adapt to the demand for higher energy density, it is urgent to develop new cathode materials with higher specific capacity, lower cost, and non-toxicity.
[0003] Compared with inorganic materials, organic materials are composed of naturally abundant elements such as C, H, N, O and S, etc. They are rich in raw materials, low in cost, green and environmentally friendly, and have flexible molecular designability and multiple redox active centers. They usually have high theoretical specific capacity and are considered to be one of the excellent candidates for low-cost and sustainable lithium-ion battery electrode materials. Nowadays, organic electrode materials including carbonyl compounds, conductive polymers, organic sulfur compounds and organic free radicals are widely used in lithium-ion batteries. However, organic electrode materials usually have problems such as easy solubility in organic electrolytes and poor inherent conductivity, resulting in low actual capacity and poor cycle performance, which greatly limits their practical application. Therefore, it is of great significance to design and develop organic cathode materials with high conductivity, good rate performance and cycle performance, and insolubility in organic electrolytes. Summary of the invention
[0004] In order to overcome the problems existing in the above-mentioned prior art, one of the purposes of the present invention is to provide an organic polymer electrode material. The second purpose of the present invention is to provide a method for preparing the above-mentioned organic polymer electrode material. The third purpose of the present invention is to provide an application of the above-mentioned organic polymer electrode material. The fourth purpose of the present invention is to provide a lithium ion battery.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides an organic polymer electrode material. The organic polymer electrode material is a polymer containing a tripyridylene structural unit, with a conjugated carbonyl group as a connecting group, and its structural formula is shown in formula (I):
[0007]
[0008] Wherein, R is a conjugated carbonyl group.
[0009] Preferably, said R is selected from One of the .
[0010] More preferably, the structural formula of the organic polymer electrode material is as shown in the following formula (I) to formula (IV):
[0011]
[0012] The second aspect of the present invention provides a method for preparing the organic polymer electrode material according to the first aspect, comprising the following steps:
[0013] Tribromotripyridinium monomer The organic polymer electrode material is prepared by polymerizing the NH2-R-NH2 monomer, wherein the NH2-R-NH2 monomer contains a diamino group and a conjugated carbonyl group.
[0014] Preferably, the tribromotripyridylene monomer is prepared by a preparation method comprising the following steps: cyclohexanone octahydrate and 4-bromo-1,2-phenylenediamine are reacted to prepare the tribromotripyridylene monomer.
[0015] More preferably, the reaction temperature of the reaction is 100-140° C., and the reaction time is 20-28 h.
[0016] More preferably, the molar ratio of the cyclohexanone octahydrate to 4-bromo-1,2-phenylenediamine is 1:(3-4).
[0017] More preferably, the reaction is carried out in a protective atmosphere.
[0018] More preferably, the cyclohexanone octahydrate and 4-bromo-1,2-phenylenediamine are reacted in glacial acetic acid solvent to obtain the tribromotripyridinium monomer.
[0019] Preferably, the method comprises the following steps: in the presence of a palladium catalyst, a biphenyl monophosphine ligand and a base, a tribromotripyridinium monomer and a monomer containing a diamino group and a conjugated carbonyl group are polymerized to obtain the organic polymer electrode material.
[0020] More preferably, the palladium catalyst is selected from one of Pd(dba)2, Pd(OAc)2 or a combination thereof.
[0021] More preferably, the molar ratio of the palladium catalyst to the tribromotripyridinium monomer is (0.03-0.1):1.
[0022] More preferably, the biphenyl monophosphine ligand is selected from one or more of XPhos, RuPhos, tBuXPhos, SPhos, XPhos, and JohnPhos.
[0023] More preferably, the molar ratio of the biphenyl monophosphine ligand to the tribromotripyridinium monomer is (0.08-0.15):1.
[0024] More preferably, the base is selected from one of t-BuOK, t-BuONa or a combination thereof.
[0025] More preferably, the molar ratio of the base to the tribromotripyridinium monomer is (2-4):1.
[0026] Preferably, the polymerization reaction is carried out under a protective atmosphere.
[0027] More preferably, the composition of the protective atmosphere includes at least one of nitrogen, helium and argon.
[0028] Preferably, the reaction temperature of the polymerization reaction is 100-140°C.
[0029] More preferably, the reaction temperature of the polymerization reaction is 110-130°C.
[0030] Preferably, the reaction time of the polymerization reaction is 72 to 120 hours.
[0031] More preferably, the reaction time of the polymerization reaction is 84 to 108 hours.
[0032] More preferably, the reaction time of the polymerization reaction is 90 to 102 hours.
[0033] Preferably, the molar ratio of the tribromotripyridinium monomer to the monomer containing a diamino group and a conjugated carbonyl group is 1:(1-2).
[0034] More preferably, the molar ratio of the tribromotripyridylene monomer to the monomer containing a diamino group and a conjugated carbonyl group is 1:(1.3-1.7).
[0035] Preferably, the polymerization reaction is carried out in a solvent, and the solvent is selected from one of toluene, xylene, THF, DME, 1,4-dioxane, DMF, NMP, and DMSO.
[0036] Preferably, the method further comprises the following steps: after the polymerization reaction, adding dilute hydrochloric acid and tetrahydrofuran and stirring for 4 to 6 hours.
[0037] The third aspect of the present invention provides use of the organic polymer electrode material of the first aspect in a lithium ion battery.
[0038] The fourth aspect of the present invention provides a lithium-ion battery, comprising a positive electrode and a negative electrode; the active material of the positive electrode comprises the organic polymer electrode material described in the first aspect.
[0039] Preferably, the positive electrode is prepared by a preparation method comprising the following steps: the organic polymer electrode material, conductive additive and binder are uniformly dispersed in a solvent, uniformly coated on a current collector, and dried to form a positive electrode film to obtain a positive electrode.
[0040] The beneficial effects of the present invention are:
[0041] The present invention provides an organic polymer electrode material, which is an organic conjugated polymer based on hexaazanaphthyl and conjugated carbonyl formed by connecting aromatic amines. The organic positive electrode material contains a nitrogen-rich conjugated structure and abundant C=N and C=O groups as active sites for lithium storage, and has excellent structural stability and high theoretical specific capacity. The theoretical specific capacity is greater than 300 mAh·g -1 When the organic polymer electrode material provided by the present invention is applied to the positive electrode of a lithium-ion battery, it achieves high specific capacity, good rate performance and cycle performance, and is expected to be applied in the field of next-generation sustainable, environmentally friendly, high-energy-density energy storage batteries.
[0042] Specifically, compared with the prior art, the present invention has the following advantages:
[0043] (1) The organic polymer electrode material provided by the present invention is an organic polymer material that does not contain transition metals, has abundant raw materials, low cost, is green and environmentally friendly, and has flexible molecular designability and multiple redox active centers.
[0044] (2) The organic polymer electrode material provided by the present invention has a π-conjugated system and a polyaniline-like structure, which is beneficial to expand the π electron delocalization and facilitate the rapid transfer of electrons, thereby improving the structural stability and rate performance of the material, effectively reducing the dissolution of the organic material in the organic electrolyte and improving the conductivity of the material to a certain extent.
[0045] (3) The organic polymer electrode material provided by the present invention has multiple redox active sites, with abundant C=N and C=O groups as active sites for lithium storage, which is beneficial to improving the theoretical specific capacity of the organic material; thereby solving the technical problems of the existing organic electrode materials for lithium-ion batteries, such as low capacity, easy solubility in organic electrolytes, and poor inherent conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 The Fourier transform infrared spectra of the products of Examples 1-4 are shown in FIG. 1 , wherein (a) is HATN-AQ; (b) is HATN-BQ; (c) is HATN-CBD; and (d) is HATN-PTO.
[0047] Figure 2 The solid-state NMR spectra of the products of Examples 1-4; wherein (a) is HATN-AQ; (b) is HATN-BQ; (c) is HATN-CBD; and (d) is HATN-PTO;
[0048] Figure 3 The rate performance diagram of the half-cell made based on the products of Examples 1-4 at different current densities;
[0049] Figure 4 The half-cell made based on the product of Example 1 was -1 The charge and discharge curve diagram when
[0050] Figure 5 The half-cell made based on the product of Example 1 was -1 Cycle performance diagram when
[0051] Figure 6 This is a rate performance diagram of a full battery made based on the product of Example 4 at different current densities;
[0052] Figure 7 The full battery made based on the product of Example 4 was -1 Cycle performance diagram when . DETAILED DESCRIPTION
[0053] The present invention is further described in detail below through specific examples. The raw materials used in the following examples, unless otherwise specified, can be obtained from conventional commercial sources or prepared and separated by simple synthesis; the processes used, unless otherwise specified, are conventional processes in the art.
[0054] Example 1
[0055] This embodiment provides an organic polymer electrode material, and the specific preparation steps are as follows:
[0056]
[0057] S1. Mix 0.94 g (3.01 mmol) of cyclohexanone octahydrate and 1.69 g (9.03 mmol) of 4-bromo-1,2-phenylenediamine, evacuate with a vacuum pump, and backfill with nitrogen. Add 50 mL of glacial acetic acid, evacuate with a vacuum pump, and backfill with nitrogen, and repeat three times. Reflux at 120 ° C for 24 h under a nitrogen atmosphere. After the reaction is completed, cool to room temperature, vacuum filter, wash with water and ethanol, and vacuum dry to obtain tribromotripyridinium (HATN-Br);
[0058] S2. Tribromotripyridinium (124 mg, 0.20 mmol), 2,6-diaminoanthraquinone (71.4 mg, 0.30 mmol), Pd(dba)2 (7.3 mg, 0.013 mmol), XPhos (10.7 mg, 0.022 mmol) and t-BuONa (50.7 mg, 0.53 mmol) were added to a 50 mL reaction tube in sequence. The reaction tube was evacuated and then backfilled with nitrogen. DMF (9 mL) was added as a solvent under a nitrogen atmosphere. The obtained mixed solution was evacuated and backfilled with nitrogen for three cycles, and then heated to 120°C for four days. After the reaction was completed, dilute hydrochloric acid and tetrahydrofuran were added and stirred for 5 hours. The obtained solution was filtered under reduced pressure and washed with water, tetrahydrofuran and anhydrous ethanol in sequence. The collected solid product was placed in a vacuum drying oven and dried overnight at 40°C to obtain a black product, i.e., the organic polymer electrode material, recorded as HATN-AQ.
[0059] Example 2
[0060] This embodiment provides an organic polymer electrode material, and the specific preparation steps are as follows:
[0061]
[0062] S1. Mix 0.94 g of cyclohexanone octahydrate and 1.69 g of 4-bromo-1,2-phenylenediamine, evacuate with a vacuum pump, and backfill with nitrogen. Add 50 mL of glacial acetic acid, evacuate with a vacuum pump, and backfill with nitrogen, and repeat three times. Reflux at 120 ° C for 24 h under a nitrogen atmosphere. After the reaction is completed, cool to room temperature, vacuum filter, wash with water and ethanol, and vacuum dry to obtain tribromotripyridinium (HATN-Br);
[0063] S2. Tribromotripyridinium chloride (124 mg, 0.20 mmol), 2,5-diaminobenzoquinone (41.4 mg, 0.30 mmol), Pd(dba)2 (7.3 mg, 0.013 mmol), XPhos (10.7 mg, 0.022 mmol) and t-BuONa (50.7 mg, 0.53 mmol) were added to a 50 mL reaction tube in sequence. The reaction tube was evacuated and then backfilled with nitrogen. DMF (9 mL) was added as a solvent under a nitrogen atmosphere. The obtained mixed solution was evacuated and backfilled with nitrogen for three cycles, and then heated to 120°C for four days. After the reaction was completed, dilute hydrochloric acid and tetrahydrofuran were added and stirred for 5 hours. The obtained solution was filtered under reduced pressure and washed with water, tetrahydrofuran and anhydrous ethanol in sequence. The collected solid product was placed in a vacuum drying oven and dried overnight at 40°C to obtain a black product, i.e., the organic polymer electrode material, recorded as HATN-BQ.
[0064] Example 3
[0065] This embodiment provides an organic polymer electrode material, and the specific preparation steps are as follows:
[0066]
[0067] S1. Mix 0.94 g of cyclohexanone octahydrate and 1.69 g of 4-bromo-1,2-phenylenediamine, evacuate with a vacuum pump, and backfill with nitrogen. Add 50 mL of glacial acetic acid, evacuate with a vacuum pump, and backfill with nitrogen, and repeat three times. Reflux at 120 ° C for 24 h under a nitrogen atmosphere. After the reaction is completed, cool to room temperature, vacuum filter, wash with water and ethanol, and vacuum dry to obtain tribromotripyridinium (HATN-Br);
[0068] S2. Tribromotripyridinium chloride (124 mg, 0.20 mmol), 3,4-diaminocyclobut-3-ene-1,2-dione (33.6 mg, 0.30 mmol), Pd(dba)2 (7.3 mg, 0.013 mmol), XPhos (10.7 mg, 0.022 mmol) and t-BuONa (50.7 mg, 0.53 mmol) were added to a 50 mL reaction tube in sequence. The reaction tube was evacuated and then backfilled with nitrogen. DMF (9 mL) was added as a solvent under a nitrogen atmosphere. The obtained mixed solution was evacuated and backfilled with nitrogen for three cycles, and then heated to 120°C for four days. After the reaction was completed, dilute hydrochloric acid and tetrahydrofuran were added and stirred for 5 hours. The obtained solution was filtered under reduced pressure and washed with water, tetrahydrofuran and anhydrous ethanol in sequence. The collected solid product was placed in a vacuum drying oven and dried overnight at 40°C to obtain a black product, i.e., the organic polymer electrode material, recorded as HATN-CBD.
[0069] Example 4
[0070] This embodiment provides an organic polymer electrode material, and the specific preparation steps are as follows:
[0071]
[0072] S1. Mix 0.94 g of cyclohexanone octahydrate and 1.69 g of 4-bromo-1,2-phenylenediamine, evacuate with a vacuum pump, and backfill with nitrogen. Add 50 mL of glacial acetic acid, evacuate with a vacuum pump, and backfill with nitrogen, and repeat three times. Reflux at 120 ° C for 24 h under a nitrogen atmosphere. After the reaction is completed, cool to room temperature, vacuum filter, wash with water and ethanol, and vacuum dry to obtain tribromotripyridinium (HATN-Br);
[0073] S2. Tribromotripyridinium (124 mg, 0.20 mmol), 2,7-diaminopyrene-4,5,9,10-tetraketone (87.7 mg, 0.30 mmol), Pd(dba)2 (7.3 mg, 0.013 mmol), XPhos (10.7 mg, 0.022 mmol) and t-BuONa (50.7 mg, 0.53 mmol) were added to a 50 mL reaction tube in sequence, and the reaction tube was evacuated and then backfilled with nitrogen. , and then DMF (9 mL) was added as a solvent under a nitrogen atmosphere; the obtained mixed solution was evacuated-backfilled with nitrogen, and the cycle was repeated three times, and then heated to 120°C for four days; after the reaction, dilute hydrochloric acid and tetrahydrofuran were added and stirred for 5 hours, the obtained solution was filtered under reduced pressure, washed with water, tetrahydrofuran and anhydrous ethanol in turn, and the collected solid product was placed in a vacuum drying oven and dried at 40°C overnight to obtain a black product, i.e., the organic polymer electrode material, recorded as HATN-PTO.
[0074] Material characterization
[0075] The organic polymers prepared in Examples 1-4 were subjected to Fourier transform infrared spectroscopy and solid nuclear magnetic resonance characterization. The results are as follows: Figure 1 and Figure 2 shown.
[0076] Figure 1 The Fourier transform infrared spectra of the products of Examples 1-4 are shown in FIG. Figure 1 As shown, HATN-3Br at 665cm -1 There is a strong stretching vibration absorption peak of the C-Br bond at 3100-3500cm. When the reaction is over, the absorption peak of the C-Br bond almost disappears, proving that the C-Br bond breaks during the reaction. At the same time, the monomers containing diamino groups (AQ-2NH2, BQ-2NH2, CBD-2NH2, PTO-2NH2) have a strong stretching vibration absorption peak at 3100-3500cm -1There is an obvious stretching vibration absorption peak of the -NH bond at the reaction site. When the reaction is completed, the absorption peak of the -NH bond almost completely disappears, and new C=O bonds, C=N bonds and CN bonds appear in the products of Examples 1-4. The above proves the successful synthesis of the aromatic amine linker and the completion of the polymerization reaction.
[0077] Figure 2 is the solid NMR spectrum of the product of Example 1-4, such as Figure 2 As shown, at approximately 180 ppm, the products of Examples 1-4 all showed obvious peaks of C=O functional groups, while the peak at approximately 140-150 ppm corresponded to CNH bonds, further verifying the successful synthesis of the aromatic amine linker and the completion of the polymerization reaction.
[0078] Experimental testing
[0079] 1. The organic positive electrode for a lithium ion battery is prepared according to the following steps: the organic polymers prepared in Examples 1-4, Ketjen black (600JD), and PVDF are respectively ground in a mortar and evenly mixed, and then NMP solvent is added, and grinding is continued to obtain an electrode slurry having a metallic luster and uniform surface, and the obtained electrode slurry is coated on a carbon-coated aluminum foil, and then dried in a 65° C. forced air drying oven for 6 h, and then transferred to a 65° C. vacuum drying oven and dried for 6 to 10 h to obtain an organic positive electrode sheet for a lithium ion battery.
[0080] A CR2032 button half-cell was assembled using metallic lithium as the negative electrode, Celgard 2325 as the separator, 1M LiTFSI, DOL:DME=1:1 (v:v), and 1% LiNO3 as the electrolyte.
[0081] The pre-lithiated graphite electrode was used as the negative electrode, Celgard 2325 was used as the separator, 1M LiPF6, EC:DEC=1:1 (v:v), and 5% FEC was used as the electrolyte to assemble a CR2032 type button-type full battery.
[0082] 2. Conduct electrochemical performance tests on the prepared button cells. Figure 3 The rate performance diagram of half-cells made of organic cathode materials HATN-AQ, HATN-BQ, HATN-CBD or HATN-PTO at different current densities shows that HATN-PTO has the best rate performance, even at 20A·g -1 At a high current density of 208.7 mAh g -1 High discharge capacity. Figure 4 The half-cell made of HATN-AQ is 0.2A·g -1 Charge and discharge curves at current density. Figure 5 The half-cell made of HATN-AQ is 5A·g-1 Cyclic performance diagram at a current density of 131.2 mAh g after 1000 cycles -1 The discharge specific capacity has good cycle stability. Figure 6 The rate performance diagram of the full battery made of HATN-PTO at different current densities. -1 227.3mAh g -1 High discharge capacity, even at 5A·g -1 At a high current density of 107.2 mAh g -1 The discharge capacity. Figure 7 The full battery made of HATN-PTO is 0.5A·g -1 Cyclic performance diagram at a current density of 1.3 Å, which still has 99.1 mAh g after 200 cycles -1 The discharge specific capacity has good cycle stability.
[0083] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An organic polymer electrode material, characterized in that: The organic polymer electrode material is a polymer containing a tripyridylene structural unit, with a conjugated carbonyl group as a connecting group, and its structural formula is shown in formula (I): Wherein, R is a conjugated carbonyl group.
2. The organic polymer electrode material according to claim 1, characterized in that: The R is selected from One of the .
3. The method for preparing the organic polymer electrode material according to claim 1 or 2, characterized in that: The steps include: Tribromotripyridinium monomer The organic polymer electrode material is prepared by polymerizing the NH2-R-NH2 monomer, wherein the NH2-R-NH2 monomer contains a diamino group and a conjugated carbonyl group.
4. The method for preparing an organic polymer electrode material according to claim 3, characterized in that: The tribromotripyridinium monomer is prepared by a preparation method comprising the following steps: cyclohexanone octahydrate and 4-bromo-1,2-phenylenediamine are reacted to prepare the tribromotripyridinium monomer.
5. The method for preparing an organic polymer electrode material according to claim 3, characterized in that: The steps include: In the presence of a palladium catalyst, a biphenyl monophosphine ligand and a base, a tribromotripyridinium monomer and an NH2-R-NH2 monomer undergo a polymerization reaction to prepare the organic polymer electrode material.
6. The method for preparing an organic polymer electrode material according to claim 3, characterized in that: The polymerization reaction was carried out under a protective atmosphere.
7. The method for preparing an organic polymer electrode material according to claim 3, characterized in that: The reaction temperature of the polymerization reaction is 100-140°C.
8. The method for preparing an organic polymer electrode material according to claim 3, characterized in that: The molar ratio of the tribromotripyridinium monomer to the monomer containing diamino group and conjugated carbonyl group is 1:(1-2).
9. Use of the organic polymer electrode material according to claim 1 or 2 in lithium ion batteries.
10. A lithium ion battery, characterized in that: It comprises a positive electrode and a negative electrode; the active material of the positive electrode comprises the organic polymer electrode material according to claim 1 or 2.
Citation Information
Patent Citations
Carbonyl-based porous organic polymer as well as preparation method and application thereof
CN115521454A
Hexaaza-trinaphthalene monomer and preparation method thereof, porous organic polymer and preparation method and application thereof
CN115557955A
Method for preparing positive electrode of lithium ion battery
WO2019001047A1