Self-foaming-self-crosslinking silicone rubber and preparation method thereof

By using self-foaming-self-crosslinking process in the preparation of silicone rubber, using water to generate CO2 to achieve foaming and crosslinking, the problems of poor performance and unenvironmental protection of traditional foamed silicone rubber are solved, and high-performance, safe and environmentally friendly silicone is obtained Rubber material.

CN118930862AInactive Publication Date: 2024-11-12NANCHANG L LIANG IND
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410572475.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

There are problems of poor performance and unenvironmental protection in the preparation process of traditional foamed silicone rubber, especially the chemical foaming method requires additional foaming agent and crosslinking agent, which is complicated in operation and has safety risks.

Method used

Using a self-foaming-self-crosslinking silicone rubber and its preparation method, foaming and crosslinking are achieved by mixing the cyclic monomer with isocyanate silane monomer at room temperature and reacting at a specific temperature. The need for additional foaming agents and crosslinking agents is avoided, and the self-foaming-self-crosslinking process is realized.

Benefits of technology

It realizes the preparation of self-foaming-self-crosslinked silicone rubber with high density, high elongation and high strength. The process is safe and environmentally friendly, and does not produce dangerous gases or polluted gases. The process is simple and the foaming ratio can be adjusted.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930862A_ABST
    Figure CN118930862A_ABST
Patent Text Reader

Abstract

The invention discloses self-foaming-self-crosslinking silicone rubber and a preparation method thereof.The method comprises the steps that at the room temperature, a plurality of cyclic monomers and a plurality of molecular weight control agents are mixed and added into a reactor, and a raw material system is obtained; the preparation method comprises the following steps: adding a plurality of isocyanate silane monomers into a raw material system, adding a first catalyst, heating to 90-140 DEG C, reacting for 4-6 hours, regulating the pH value of the system to be neutral, removing low-boiling-point substances in vacuum, and adding a second catalyst to obtain a self-foaming-self-crosslinking silicone rubber precursor; and mixing the self-foaming-self-crosslinking silicone rubber precursor with water, and foaming at 60-80 DEG C for 15-60 minutes to obtain a self-foaming-self-crosslinking silicone rubber finished product. The self-foaming-self-crosslinking silicone rubber prepared by the invention has the advantages of high density, high strength and high elongation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of foaming silicone rubber preparation, and in particular to a self-foaming and self-cross-linking silicone rubber and a preparation method thereof. Background Art

[0002] As a special form of silicone rubber material, foamed silicone rubber is a porous polymer elastomer after foaming. Due to its special structure, silicone rubber itself has good high and low temperature resistance, flame retardant properties and physiological inertness, while foam materials have the characteristics of light weight, good cushioning and shock absorption, damping sound insulation and thermal insulation. Therefore, foamed silicone rubber materials have the advantages of both ordinary silicone rubber and foamed materials, making them widely used in national defense, military industry and daily life. Foreign research and development and application in the field of foamed silicone rubber began in the above. According to the different foaming mechanisms, foamed silicone rubber can be divided into physical foaming and chemical foaming.

[0003] There are also many forms of physical foaming of silicone rubber. Inert gas (CO2, hydrogen, etc.) or low-boiling liquid (halogenated hydrocarbons, alkanes, etc.) can be mixed into silicone rubber by stirring or pressurizing. After cross-linking and curing reaction, the gas inside can be removed by decompression and heating to achieve the physical foaming effect of silicone rubber. Bai Jianwei et al. used supercritical carbon dioxide physical foaming agent to prepare carbon nanotube modified silicone rubber composite materials, which improved the density and uniformity of the pore structure and improved the mechanical properties and electrical conductivity of the foam material. Lixian Song et al. used supercritical carbon dioxide to prepare foamed silicone rubber and studied the effect of pre-vulcanization time on the cross-linked network structure. The results showed that under the condition of pre-vulcanization for 5 minutes, the foaming effect was the best, the sample density was the lowest at 0.239g / cm3, and the prepared foam had an interconnected polygonal pore structure. However, inert gases are difficult to store in polymers for a long time at room temperature, and the gas must be introduced before foaming, which is inconvenient to operate; low-boiling point liquids are usually halogenated hydrocarbons or liquid alkanes. The former has a destructive effect on the ozone layer, and the latter is flammable, explosive and unsafe.

[0004] The chemical foaming method of silicone rubber refers to the chemical reaction of silicone rubber during the foaming process, including external foaming and internal foaming. The external foaming agent method is because in the preparation process of silicone rubber, a substance that can decompose and release gas under heat is added from the outside. Common foaming agents include AC (azodicarbonamide), OBSH (4,4'-oxybisbenzenesulfonylhydrazine) H (N,N-dinitrosopentamethinetetramine), sodium bicarbonate, etc. The external foaming method requires strict control of the amount of foaming agent to match it with the cross-linking reaction in order to achieve a good foaming effect. In special cases, a suitable foaming aid must be selected. Ding Guofang et al. used H (N,N-dinitrosopentamethinetetramine) as a foaming agent and urea as a foaming aid. The two cooperated with each other in a mass ratio of 1:1 to prepare foam silicone rubber with good performance. However, conventional chemical foaming requires both a foaming agent and a cross-linking agent, making it difficult to achieve the dual purpose of foaming and cross-linking. The foaming temperature of the foaming agent and the cross-linking temperature of the cross-linking agent need to match in order to successfully obtain a foamed rubber with better performance. The operation is difficult, limiting its scope of application.

[0005] The internal foaming principle refers to the chemical reaction between the raw material components of the silicone rubber, which releases a large amount of gas from the inside of the system to achieve the purpose of foaming. This method can form a silicone rubber material with a uniform pore structure without external heating conditions, and a cross-linking reaction to form a network structure occurs at the same time, which has attracted widespread attention from scientific researchers in recent years. The common mechanism in chemical foaming is that under the condition of platinum catalyst, dihydroxy polydimethylsiloxane and hydrogen-containing silicone oil undergo a silylation dehydrogenation reaction, and the generated hydrogen promotes the formation of a pore structure; terminal vinyl polydimethylsiloxane and hydrogen-containing silicone oil undergo a silylation addition reaction, and a network structure is gradually formed inside, and finally a foamy or spongy silicone rubber elastomer is prepared. However, this type of method will produce relatively dangerous H2, which is easy to cause production safety accidents. Therefore, it is urgent to prepare a safe, reliable, environmentally friendly, and self-foaming-self-crosslinking foaming silicone rubber. Summary of the invention

[0006] The purpose of this application is to propose a self-foaming and self-cross-linking silicone rubber and a preparation method thereof, aiming to provide a new type of self-foaming and self-cross-linking foaming silicone rubber synthesized by a new process, so as to solve the technical problems of poor performance and environmentally unfriendly preparation process of foaming silicone rubber obtained by traditional synthesis method.

[0007] On the one hand, the present application proposes a self-foaming and self-crosslinking silicone rubber having both a polysiloxane segment structure and an isocyanate structure, and its structural formula is as follows:

[0008]

[0009] Wherein, n is 20 to 100, m is 500 to 1000, R1 is vinyl or methyl, and R2 is methyl ether or methyl.

[0010] On the other hand, the present application also proposes a method for preparing a self-foaming-self-crosslinking silicone rubber, the preparation method comprising:

[0011] At room temperature, a plurality of cyclic monomers and a plurality of molecular weight control agents are mixed and added into a reactor to obtain a raw material system;

[0012] Add a certain amount of isocyanate silane monomers and a first catalyst to the raw material system, heat to 90-140°C and react for 4-6 hours, adjust the pH of the system to neutral, remove low-boiling substances in vacuum, add a second catalyst, and obtain a self-foaming and self-crosslinking silicone rubber precursor;

[0013] The self-foaming and self-cross-linking silicone rubber precursor is mixed with water, and foamed at 60 to 80° C. for 15 to 60 minutes to obtain a self-foaming and self-cross-linking silicone rubber product.

[0014] According to the above preparation method, the isocyanate structure is introduced into the silicone rubber macromolecule, and the isocyanate is used to react with water to produce CO2 and -NH2. CO2 is used as a non-flammable foaming gas to complete the foaming process, and -NH2 is used as a cross-linking agent to continue to react with the isocyanate to produce a urea structure and chemical cross-linking. The entire foaming and cross-linking process only requires the addition of water, without the need to add additional foaming agents and cross-linking agents, to achieve the "one-dose two-purpose" self-foaming-self-cross-linking process of foaming-cross-linking, and obtain a new type of self-foaming-self-cross-linking silicone rubber with high density, high elongation, and high strength. In addition, the entire foaming-cross-linking process does not produce halogenated hydrocarbons that harm the ozone layer, nor does it produce dangerous hydrogen, which is safe and environmentally friendly.

[0015] In some preferred embodiments, the cyclic monomer is at least one of octamethylcyclotetrasiloxane, hexamethylcyclotrisiloxane, and decamethylcyclopentasiloxane.

[0016] In some preferred embodiments, the isocyanate silane monomer is at least one of isocyanate propyl trimethoxy silane and isocyanate propyl methyl dimethoxy silane.

[0017] In some preferred embodiments, the molecular weight control agent is at least one of hexamethyldisiloxane and divinyltetramethyldisiloxane.

[0018] In some preferred embodiments, the first catalyst is at least one of dibutyltin dilaurate, dibutylbismuth dilaurate, triethylenediamine, and N-methylmorpholine, and the second catalyst is at least one of dibutyltin dilaurate, dibutylbismuth dilaurate, triethylenediamine, and N-methylmorpholine.

[0019] In some preferred embodiments, the molar ratio of the cyclic monomer to the molecular weight control agent is 500:1 to 1000:1.

[0020] In some preferred embodiments, the ratio of the isocyanate silane monomer to the cyclic monomer is 1:50 to 1:5.

[0021] In some preferred embodiments, the mass ratio of the self-foaming-self-cross-linking silicone rubber precursor to the water is 100:40 to 100:5.

[0022] Compared with the prior art, this application has the following advantages:

[0023] 1. The preparation process proposed in this application does not require the addition of foaming agents and cross-linking agents as in the traditional process. The self-foaming-self-cross-linking process can be generated by mixing a homemade silicone rubber precursor with water;

[0024] 2. The entire preparation process of the present application does not produce polluting gases, such as halogenated hydrocarbons, nor does it produce dangerous explosive gases, such as hydrogen, which is safer and more environmentally friendly than traditional preparation processes;

[0025] 3. The foaming process in the preparation process proposed in this application is simple and only requires water, and the foaming ratio can be adjusted according to the amount of water used, and can be flexibly adjusted according to different usage requirements.

[0026] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become apparent from the following description, or will be understood through the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A flow chart of a method for preparing a self-foaming and self-crosslinking silicone rubber precursor according to an embodiment of the present application is shown;

[0028] Figure 2 The 1H-NMR result diagram of the structure of the self-foaming and self-crosslinking silicone rubber precursor prepared in Example 6 is shown;

[0029] Figure 3 The FT-IR result diagram of the self-foaming and self-cross-linking silicone rubber precursor prepared in Example 6 is shown. DETAILED DESCRIPTION

[0030] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Several embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0032] Embodiment 1

[0033] Step S11, mixing raw materials: at room temperature, mixing the cyclic monomer (octamethylcyclotetrasiloxane) and the molecular weight control agent (hexamethyldisiloxane) into a reactor, wherein the molar ratio of the cyclic monomer to the molecular weight control agent is 500:1;

[0034] Step S12, preparation of precursor: add isocyanate silane monomer (isocyanate propyl trimethoxy silane) to the system of step S11, then add catalyst (sodium hydroxide) and stir evenly, heat to 90°C and react for 4 hours, adjust the pH of the system to neutral, remove low boiling points in vacuo, add catalyst (dibutyltin dilaurate), and obtain self-foaming-self-crosslinking silicone rubber precursor. The ratio of isocyanate silane monomer to cyclic monomer is 1:5, and the amount of both catalysts is 0.5% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

[0035] Step S13, mixing the self-foaming-self-crosslinking silicone rubber precursor in step S12 with water, and foaming at 60°C for 15 minutes to obtain a self-foaming-self-crosslinking silicone rubber product. The mass ratio of the self-foaming-self-crosslinking silicone rubber precursor to water is 100:5, and the obtained self-foaming-self-crosslinking silicone rubber product has the structural formula:

[0036]

[0037] Embodiment 2

[0038] Step S11, mixing raw materials: at room temperature, mixing a cyclic monomer (hexamethylcyclotrisiloxane) and a molecular weight control agent (divinyltetramethyldisiloxane) and adding them into a reactor, wherein the molar ratio of the cyclic monomer to the molecular weight control agent is 1000:1;

[0039] Step S12, preparation of precursor: add isocyanate silane monomer (isocyanate propylmethyldimethoxysilane) to the system of step S11, then add catalyst (potassium hydroxide) and stir evenly, heat to 140°C and react for 6 hours, adjust the pH of the system to neutral, remove low boiling points in vacuo, add catalyst (dibutyl bismuth dilaurate), and obtain self-foaming-self-crosslinking silicone rubber precursor. The ratio of isocyanate silane monomer to cyclic monomer is 1:50, and the amount of both catalysts is 0.5% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

[0040] Step S13, mixing the self-foaming-self-crosslinking silicone rubber precursor in step S12 with water, and foaming at 80°C for 60 minutes to obtain a self-foaming-self-crosslinking silicone rubber product. The mass ratio of the self-foaming-self-crosslinking silicone rubber precursor to water is 100:40, and the obtained self-foaming-self-crosslinking silicone rubber product has the structural formula:

[0041]

[0042] Embodiment 3

[0043] Step S11, mixing raw materials: at room temperature, mixing the cyclic monomer (decamethylcyclopentasiloxane) and the molecular weight control agent (hexamethyldisiloxane) into a reactor, wherein the molar ratio of the cyclic monomer to the molecular weight control agent is 600:1;

[0044] Step S12, preparation of precursor: add isocyanate silane monomer (isocyanate propyl trimethoxy silane) to the system of step S11, then add catalyst (one or more of tetramethyl ammonium hydroxide) and stir evenly, heat to 100°C and react for 5 hours, adjust the pH of the system to neutral, remove low boiling points in vacuo, add catalyst (triethylenediamine), and obtain self-foaming-self-crosslinking silicone rubber precursor. The ratio of isocyanate silane monomer to cyclic monomer is 1:10, and the amount of both catalysts is 1% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

[0045] Step S13, mixing the self-foaming and self-crosslinking silicone rubber precursor in step S12 with water, and foaming at 70°C for 20 minutes to obtain a self-foaming and self-crosslinking silicone rubber product. The mass ratio of the self-foaming and self-crosslinking silicone rubber precursor to water is 100:10, and the obtained self-foaming and self-crosslinking silicone rubber product has the structural formula:

[0046]

[0047] Embodiment 4

[0048] Step S11, raw material mixing: at room temperature, a cyclic monomer (octamethylcyclotetrasiloxane) and a molecular weight control agent (hexamethyldisiloxane) are mixed and added into a reactor, wherein the molar ratio of the cyclic monomer to the molecular weight control agent is 700:1;

[0049] Step S12, preparation of precursor: add isocyanate silane monomer (isocyanate propylmethyldimethoxysilane) to the system of step S11, then add catalyst (in tetramethylammonium hydroxide) and stir evenly, heat to 110°C and react for 4 hours, adjust the pH of the system to neutral, remove low boiling points in vacuo, add catalyst (N-methylmorpholine), and obtain self-foaming-self-crosslinking silicone rubber precursor. The ratio of isocyanate silane monomer to cyclic monomer is 1:15, and the amount of both catalysts is 1.5% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

[0050] Step S13, mixing the self-foaming-self-crosslinking silicone rubber precursor in step S12 with water, and foaming at 80°C for 25 minutes to obtain a self-foaming-self-crosslinking silicone rubber product. The mass ratio of the self-foaming-self-crosslinking silicone rubber precursor to water is 100:20, and the obtained self-foaming-self-crosslinking silicone rubber product has the structural formula:

[0051]

[0052] Embodiment 5

[0053] Step S11, raw material mixing: at room temperature, a cyclic monomer (hexamethylcyclotrisiloxane) and a molecular weight control agent (divinyltetramethyldisiloxane) are mixed and added into a reactor, wherein the molar ratio of the cyclic monomer to the molecular weight control agent is 800:1;

[0054] Step S12, preparation of precursor: add isocyanate silane monomer (isocyanate propyl trimethoxy silane) to the system of step S11, then add catalyst (potassium hydroxide) and stir evenly, heat to 130°C and react for 6 hours, adjust the pH of the system to neutral, remove low boiling points in vacuo, add catalyst (dibutyltin dilaurate, N-methylmorpholine, the mass ratio of the two is 1:1), and obtain self-foaming-self-crosslinking silicone rubber precursor. The ratio of isocyanate silane monomer to cyclic monomer is 1:40, and the amount of catalyst is 4% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

[0055] Step S13, mixing the self-foaming-self-crosslinking silicone rubber precursor in step S12 with water, and foaming at 75°C for 50 minutes to obtain a self-foaming-self-crosslinking silicone rubber product. The mass ratio of the self-foaming-self-crosslinking silicone rubber precursor to water is 100:30, and the obtained self-foaming-self-crosslinking silicone rubber product has the structural formula:

[0056]

[0057] Embodiment 6

[0058] Step S11, raw material mixing: at room temperature, a cyclic monomer (octamethylcyclotetrasiloxane, hexamethylcyclotrisiloxane, the mass ratio of the two is 1:1) and a molecular weight control agent (hexamethyldisiloxane) are mixed and added into a reactor, wherein the molar ratio of the cyclic monomer to the molecular weight control agent is 900:1;

[0059] Step S12, preparation of precursor: add isocyanate silane monomer (isocyanate propylmethyldimethoxysilane) to the system of step S11, then add catalyst (tetramethylammonium hydroxide) and stir evenly, heat to 110°C and react for 5 hours, adjust the pH of the system to neutral, remove low boiling points in vacuo, add catalyst (dibutyltin dilaurate, triethylenediamine, the mass ratio of the two is 1:1), and obtain self-foaming-self-crosslinking silicone rubber precursor. The ratio of isocyanate silane monomer to cyclic monomer is 1:20, and the amount of the two catalysts is 4% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

[0060] Step S13, mixing the self-foaming and self-crosslinking silicone rubber precursor in step S12 with water, and foaming at 75°C for 25 minutes to obtain a self-foaming and self-crosslinking silicone rubber product. The mass ratio of the self-foaming and self-crosslinking silicone rubber precursor to water is 100:30, and the obtained self-foaming and self-crosslinking silicone rubber product has the structural formula:

[0061]

[0062] Embodiment 7

[0063] Step S11, raw material mixing: at room temperature, a cyclic monomer (octamethylcyclotetrasiloxane, hexamethylcyclotrisiloxane, the mass ratio of the two is 1:1) and a molecular weight control agent (hexamethyldisiloxane) are mixed and added into a reactor, wherein the molar ratio of the cyclic monomer to the molecular weight control agent is 450:1;

[0064] Step S12, preparation of precursor: add isocyanate silane monomer (isocyanate propylmethyldimethoxysilane) to the system of step S11, then add catalyst (tetramethylammonium hydroxide) and stir evenly, heat to 110°C and react for 5 hours, adjust the pH of the system to neutral, remove low boiling points in vacuo, add catalyst (dibutyltin dilaurate, triethylenediamine, the mass ratio of the two is 1:1), and obtain self-foaming-self-crosslinking silicone rubber precursor. The ratio of isocyanate silane monomer to cyclic monomer is 1:18, and the amount of the two catalysts is 4.5% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

[0065] Step S13, mixing the self-foaming-self-crosslinking silicone rubber precursor in step S12 with water, and foaming at 75°C for 25 minutes to obtain a self-foaming-self-crosslinking silicone rubber product. The mass ratio of the self-foaming-self-crosslinking silicone rubber precursor to water is 100:25, and the obtained self-foaming-self-crosslinking silicone rubber product has the structural formula:

[0066]

[0067] Please refer to Table 1 below, which is a performance comparison table of the foamed silicone rubber products prepared in Examples 1-7 and commercially available foamed (hydrogen foamed) silicone rubber products. It can be seen from Table 1 that the preparation process proposed in the present application can be used to prepare self-foaming and self-cross-linking silicone rubbers of many different densities, that is, the density of the product can be flexibly adjusted to meet the needs of different scenarios. At the same time, the self-foaming and self-cross-linking silicone rubber obtained by the preparation process of the present application has tensile strength and elongation at break that are far superior to those of commercially available foamed (hydrogen foamed) silicone rubber products. Even when the density is similar, the tensile strength and elongation at break of the self-foaming and self-cross-linking silicone rubber of the present application are higher than those of commercially available products. In addition, the preparation process of all embodiments of the present application does not produce dangerous H2 or alkanes, and halogenated hydrocarbons that pollute the atmosphere, and has huge advantages in safety and environmental protection.

[0068] Table 1

[0069]

[0070] See also Figure 2 , which is the 1H-NMR result diagram of the structure of the self-foaming-self-crosslinking silicone rubber precursor prepared in Example 6. Figure 2 It can be seen that the chemical shift of the hydrogen atom of the methylene group connected to the isocyanate structure appears near 3.5 ppm, and the chemical shift of the silyl methyl hydrogen appears near 0.5 ppm, which indicates that the siloxane structure and the isocyanate structure are successfully introduced into the polymer structure.

[0071] See also Figure 3 , which is the FT-IR result of the self-foaming and self-crosslinking silicone rubber precursor prepared in Example 6, Figure 3 It can be seen that at 1670cm -1 The infrared absorption peak of carbonyl group in isocyanate appeared, 1000-1100cm -1 The infrared absorption peak of silicon-oxygen bond appears, combined with Figure 2 It shows that the polymer structure contains isocyanate and polysiloxane structure.

[0072] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A self-foaming and self-crosslinking silicone rubber, characterized in that: Its structural formula is as follows: Wherein, n is 20 to 100, m is 500 to 1000, R1 is vinyl or methyl, and R2 is methyl ether or methyl.

2. A method for preparing a self-foaming and self-crosslinking silicone rubber as claimed in claim 1, characterized in that: The preparation method comprises: At room temperature, a plurality of cyclic monomers and a plurality of molecular weight control agents are mixed and added into a reactor to obtain a raw material system; Add a certain amount of isocyanate silane monomers and a first catalyst to the raw material system, heat to 90-140°C and react for 4-6 hours, adjust the pH of the system to neutral, remove low-boiling substances in vacuum, add a second catalyst, and obtain a self-foaming and self-crosslinking silicone rubber precursor; The self-foaming and self-cross-linking silicone rubber precursor is mixed with water, and foamed at 60 to 80° C. for 15 to 60 minutes to obtain a self-foaming and self-cross-linking silicone rubber product.

3. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 2, characterized in that: The cyclic monomer is at least one of octamethylcyclotetrasiloxane, hexamethylcyclotrisiloxane and decamethylcyclopentasiloxane.

4. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 2, characterized in that: The isocyanate silane monomer is at least one of isocyanate propyl trimethoxy silane and isocyanate propyl methyl dimethoxy silane.

5. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 2, characterized in that: The molecular weight control agent is at least one of hexamethyldisiloxane and divinyltetramethyldisiloxane.

6. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 2, characterized in that: The first catalyst is at least one of dibutyltin dilaurate, dibutylbismuth dilaurate, triethylenediamine, and N-methylmorpholine, and the second catalyst is at least one of dibutyltin dilaurate, dibutylbismuth dilaurate, triethylenediamine, and N-methylmorpholine.

7. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 2, characterized in that: The molar ratio of the cyclic monomer to the molecular weight control agent is 500:1 to 1000:

1.

8. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 2, characterized in that: The ratio of the isocyanate silane monomer to the cyclic monomer is 1:50 to 1:

5.

9. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 2, characterized in that: The mass ratio of the self-foaming-self-crosslinking silicone rubber precursor to the water is 100:40 to 100:

5.

10. The method for preparing a self-foaming and self-crosslinking silicone rubber according to claim 6, characterized in that: The usage amount of the first catalyst and the second catalyst is 0.5%-5% of the total mass of the self-foaming-self-crosslinking silicone rubber precursor after mixing with water.

Citation Information

Patent Citations

  • Foams containing silicon

    CN101405319A

  • Silanol silicone resin and preparation method thereof

    CN109734917A

  • Closed isocyanate-based POSS and preparation method thereof

    CN113336948A

  • Silane-terminated resin for low-viscosity sealant and preparation method thereof

    CN116535636A

  • Flexible cellular material, composition and process for its preparation

    CN1232056A