Metal organic framework material with ethylene and propylene adsorption separation function and preparation method
By designing the metal organic frame material [Co2(OATA)(DPA)]·4DMF, and preparing by solvent-thermal synthesis method, the problem of insufficient separation performance between ethylene and propylene in the prior art was solved, and efficient propylene/ethylene adsorption selectivity was achieved , suitable for the separation of high-purity ethylene in chemical production.
Patent Information
- Application Number
- CN202410975625.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-19
AI Technical Summary
It is difficult to separate high-purity ethylene in the existing process, especially in low-carbon mixed olefins of propylene and ethylene. Traditional porous materials have shortcomings in adsorption and separation performance, which is difficult to meet the demand for high-purity ethylene in chemical production.
A metal organic frame material [Co2(OATA)(DPA)]·4DMF was designed, prepared by solvent thermal synthesis method. The material has a throat-like pore structure and high porosity, which optimizes the adsorption selectivity of propylene and ethylene, and uses DPA The "restricted entrance" formed by ligands significantly improves the adsorption properties of propylene.
The efficient separation of propylene and ethylene is achieved, and the adsorption selectivity of propylene/ethylene reaches 21.7-23.1. The material shows obvious preferential adsorption to propylene, and has weak adsorption effect on ethylene, which has high adsorption selectivity of propylene/ethylene, and is suitable for ethylene. High purity separation from propylene.
Smart Images

Figure CN118930878A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic and material chemistry sciences; in particular, it relates to a metal organic framework material with ethylene and propylene adsorption separation and a preparation method thereof. Background Art
[0002] Ethylene is an important raw material for the petrochemical industry. In 2022, the global total ethylene production capacity has reached nearly 220 million tons / year, of which my country's ethylene production has reached nearly 40 million tons. At present, there are mature processes for coal-to-olefins (CTO) and methanol-to-olefins (MTO), but both produce low-carbon mixed olefins mainly composed of propylene and ethylene. However, chemical production usually requires high-purity ethylene (99.5%), and ethylene purification is the key to ensure its effective use. Removing excess impurities in ethylene products has become the most critical and challenging task in the ethylene purification process.
[0003] Adsorption separation is a new technology with low energy consumption, simple process and high efficiency. It achieves separation through the difference in adsorption of different substances by adsorbents, among which adsorbents are the key. Metal-organic frameworks, referred to as MOFs (metal-organic frameworks), are porous crystalline materials formed by coordination assembly of organic ligands and metal centers. Isophthalic acid ligands can easily coordinate with multiple metal centers through carboxylic acids to form multi-core cluster building units, thereby forming MOFs materials with the desired structure. Pyridine ligands (DPA) are introduced into MOFs. The -NH- group in the DPA linker can not only form dense electronegative binding sites to increase the gas adsorption amount, but also further produce a throat-shaped "restricted entrance" for adsorbing propylene and rejecting ethylene, which will significantly improve the adsorption and separation performance of MOFs. Compared with traditional porous materials, MOFs have great advantages as adsorbents to produce high-purity ethylene. It is of great significance to design and synthesize MOFs materials for adsorption and separation of ethylene and propylene. Summary of the invention
[0004] The purpose of the present invention is to provide a metal organic framework material with ethylene and propylene adsorption separation and a preparation method.
[0005] The present invention is achieved through the following technical solutions:
[0006] The present invention relates to a metal organic framework material with ethylene and propylene adsorption and separation functions. The chemical formula of the metal organic framework material is [Co2(OATA)(DPA)]·4DMF;
[0007] In the chemical formula, OATA is deprotonated N, N'-bis(isophthalic acid)oxalamide, DPA is di(pyridin-4-yl)amine, and DMF is N, N-dimethylformamide;
[0008] Preferably, the metal organic framework material has a crystal structure of tetragonal system I422 space group, and the asymmetric unit consists of a Co 2+ ions, an OATA 4- ligand and a DPA ligand.
[0009] Preferably, the metal organic framework material has a throat-shaped pore structure and a BET specific surface area of 823.2 m 2 g -1 At 298K and 0.05 atm, the adsorption capacity of propylene and ethylene is 97.8 cm 3 ·g -1 and 20.0cm 3 ·g -1 , which is almost four times different; the separation selectivity of the material for propylene and ethylene mixture reaches 21.7-23.1, and it has good adsorption separation function.
[0010] Preferably, the structural formula of the ligand H4OATA of the metal organic framework material is as shown in formula (I):
[0011]
[0012] The structural formula of the DPA is shown in formula (II):
[0013]
[0014] The present invention also relates to a method for preparing the aforementioned metal organic framework material having the ability to adsorb and separate ethylene and propylene, comprising the following steps:
[0015] The present invention adopts a solvent thermal synthesis method, using cobalt nitrate hexahydrate, organic ligand N, N'-bis(isophthalic acid) oxalamide and di(pyridin-4-yl)amine as raw materials, and the specific steps are as follows:
[0016] Step 1, adding 0.09-0.11 mmol of cobalt nitrate hexahydrate, 0.04-0.05 mmol of N,N'-bis(isophthalic acid)oxalamide ligand and 0.04-0.05 mmol of di(pyridin-4-yl)amine ligand to a mixed solvent consisting of N,N-dimethylformamide and concentrated nitric acid to obtain a mixture;
[0017] Step 2, placing the mixture in a 15 ml autoclave, heating and keeping warm, and then cooling to room temperature at a rate of 20 to 30° C. per hour;
[0018] Step 3, taking out the reaction product, filtering it to obtain cyan flaky crystals, and obtaining a preliminary metal organic framework material;
[0019] Step 4, exchanging the preliminary metal organic framework material with acetone, and heating in vacuum to obtain a metal organic framework material having the function of adsorption and separation of ethylene and propylene.
[0020] Preferably, the mixed solvent is composed of 5-6 ml of N,N-dimethylformamide and 0.08-0.1 ml of concentrated nitric acid.
[0021] Preferably, in step 2, the temperature of the sealed heating is 115-125° C., and the insulation time is 70 to 80 hours.
[0022] Preferably, in step 4, the exchange time is 2 to 3 days.
[0023] Preferably, in step 4, the vacuum heating temperature is 150-160° C. and the time is 4-6 hours.
[0024] The present invention has the following advantages:
[0025] (1) The metal organic framework material for the adsorption separation of ethylene and propylene involved in the present invention has a simple preparation process, mild reaction conditions, and the ligand raw materials used are widely available;
[0026] (2) The porosity of the metal organic framework material prepared by the method involved in the present invention is 56.3%, containing a throat-shaped pore structure, and the minimum pore size is only 0.5 nm. The obtained metal organic framework material shows obvious preferential adsorption for propylene and weak adsorption for ethylene. Therefore, it has a high propylene / ethylene adsorption selectivity and can be used as a potential adsorption separation material in the field of adsorption separation of ethylene and propylene. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is the Co in the metal organic framework material of the present invention 2+ Coordination environment diagram of the ion;
[0028] Figure 2 is a three-dimensional structural diagram of the metal organic framework material of the present invention;
[0029] Figure 3 is a powder X-ray diffraction pattern of the metal organic framework material of the present invention;
[0030] Figure 4 is a nitrogen adsorption isotherm diagram of the metal organic framework material of the present invention at 77K;
[0031] Figure 5 is an adsorption isotherm diagram of ethylene and propylene of the metal organic framework material of the present invention at room temperature;
[0032] Figure 6This is a comparison chart of the selectivity of metal organic framework materials for ethylene / propylene mixtures with different mixing ratios at 298K and 1atm calculated using ideal adsorption solution theory. DETAILED DESCRIPTION
[0033] The present invention is described in detail below in conjunction with specific embodiments. It should be noted that the following embodiments are only further descriptions of the present invention, but the protection scope of the present invention is not limited to the following embodiments.
[0034] Example
[0035] This embodiment relates to a method for preparing a metal organic framework material capable of adsorption separation of ethylene and propylene, and the specific steps are as follows:
[0036] Step 1, 0.029 g of cobalt nitrate hexahydrate (0.10 mmol), 0.021 g of N,N'-bis(isophthalic acid)oxalamide (0.05 mmol), and 0.008 g of di(pyridin-4-yl)amine (0.05 mmol) were uniformly mixed with 5 mL of N,N-dimethylformamide (DMF) to obtain a mixture;
[0037] Step 2, placing the mixed solution in a 15 mL high pressure reactor, heating it to 120° C. for 72 hours, and then cooling it to room temperature;
[0038] Step 3, taking out the reaction product, filtering it to obtain cyan flaky crystals, and obtaining a preliminary metal organic framework material;
[0039] Step 4, exchanging the solvent of the preliminary metal organic framework material with acetone every 12 hours, for 6 times, and heating at 160° C. in vacuum for 6 hours to obtain a metal organic framework material with ethylene and propylene adsorption and separation functions.
[0040] (1) Structural description of the obtained metal organic framework material with ethylene and propylene adsorption separation
[0041] The crystal of the metal organic framework material is structurally characterized and analyzed to determine its unit cell and spatial structure. The crystal belongs to the tetragonal system I422 space group, and the asymmetric unit consists of a Co 2+ ions, an OATA 4- ligand and a DPA ligand, see Figure 1 As shown. Two Co 2+ ions and four carboxyl groups form a [Co2(COO)4] paddle wheel SBU, and each Co 2+ ions form a complex consisting of four different OATA 4- The O atom of the ligand and the N atom of one DPA form a pyramidal coordination configuration. 4-Interconnecting SBUs in a four-way connection generates a three-dimensional framework, see Figure 2 As shown. The DPA ligands occupying the vertices of SBUs support the framework and divide the pore space, giving the framework narrow pores and high stability. The pore surface is modified by -CONH- and -NH- groups. It is worth noting that in addition to the straight channel modified with oxalamide (0.68nm), the imine in the DPA ligand forms a "restrictive entrance" in the original channel, resulting in the formation of a throat-like channel in the framework. The narrow pore diameter is only 0.5nm, which is an ultramicropore. At the same time, the metal organic framework material has a high porosity of 56.3%, which ensures a higher adsorption capacity.
[0042] (2) Adsorption test of the obtained metal organic framework material with ethylene and propylene adsorption separation
[0043] The obtained metal organic framework material was subjected to solvent exchange with acetone, and the solvent was exchanged every 12 hours for 6 times, and then activated under vacuum conditions at 160°C for 6 hours to obtain the activated metal organic framework material. The powder X-ray diffraction measurement results showed that the activated metal organic framework material had a high phase purity, as shown in FIG. Figure 3 The nitrogen gas adsorption test was carried out using the ASAP 2020M specific surface area meter of the American Micromeritics Company. The BET specific surface area of the metal organic framework material was 823.2 m 2 g -1 ,See Figure 4 The adsorption and separation performance of the metal organic framework material for propylene / ethylene was then further tested. Under the conditions of 298K and 1 bar, the adsorption capacity of the material for propylene was 121.3 cm 3 g -1 , significantly higher than ethylene (94.5cm 3 g -1 ),like Figure 5 Moreover, at high temperatures of 313K and 333K, the adsorption capacity of propylene by the material at 1 bar still remained at 111.9 cm 3 g -1 and 101.9cm 3 g -1 The above test results show that the material still has good adsorption capacity in industrial processes with relatively high temperatures.
[0044] Through Figure 5 Further study of the adsorption curves in the results showed that the adsorption curve of propylene at low pressure increased rapidly, especially at 0.05 bar, the adsorption amount reached 97.8 cm 3 g -1, which is 80.6% of the adsorption capacity at 1 bar pressure and about 5 times that of ethylene, which makes the metal organic framework material show significant propylene / ethylene selectivity. Figure 6 As shown, at 0.1 bar and 1 bar, for propylene / ethylene mixtures in different ratios: for propylene / ethylene = 50 / 50 mixture, the selectivity reaches 21.9 and 23.1 respectively; for propylene / ethylene = 25 / 75 mixture, the selectivity reaches 21.7 and 22.7 respectively; for propylene / ethylene = 25 / 75 mixture, the selectivity reaches 21.6 and 22.3 respectively, showing excellent ethylene / propylene separation potential.
[0045] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which will not affect the essence of the present invention.
Claims
1. A metal organic framework material with ethylene and propylene adsorption separation, It is characterized in that The chemical formula of the metal organic framework material is [Co 2 (OATA)(DPA)]·4DMF; In the chemical formula, OATA is deprotonated N, N'-bis(isophthalic acid) oxalamide, DPA is di(pyridin-4-yl)amine, and DMF is N, N-dimethylformamide.
2. The metal organic framework material having the ability to adsorb and separate ethylene and propylene as claimed in claim 1, It is characterized in that The crystal of the metal organic framework material belongs to the tetragonal I422 space group, and the asymmetric unit consists of a Co 2+ ions, an OATA 4- ligand and a DPA ligand.
3. The metal organic framework material having the ability to adsorb and separate ethylene and propylene as claimed in claim 1, It is characterized in that The metal organic framework material has a throat-shaped pore structure and a BET specific surface area of 823.2 m 2 g -1 At 298K and 0.05 atm, the adsorption capacity of propylene and ethylene is 97.8 cm 3 ·g -1 and 20.0cm 3 ·g -1 The separation selectivity of the material for a mixture of propylene and ethylene is 21.7-23.
1.
4. The metal organic framework material having the ability to adsorb and separate ethylene and propylene as claimed in claim 2, It is characterized in that The ligand H of the metal organic framework material 4 The structural formula of OATA is shown in formula (I): The structural formula of the DPA is shown in formula (II):
5. A method for preparing a metal organic framework material having ethylene and propylene adsorption separation as claimed in claim 1, It is characterized in that The following steps are involved: Step 1, adding cobalt nitrate hexahydrate, N,N'-bis(isophthalic acid)oxalamide ligand and di(pyridin-4-yl)amine ligand into a mixed solvent consisting of N,N-dimethylformamide and concentrated nitric acid to obtain a mixture; Step 2, placing the mixture in a 15 ml autoclave, heating and keeping warm, and cooling to room temperature at a rate of 20-30° C. per hour; Step 3, taking out the reaction product, filtering it to obtain cyan flaky crystals, and obtaining a preliminary metal organic framework material; Step 4, exchanging the preliminary metal organic framework material with acetone, and heating in vacuum to obtain a metal organic framework material having the function of adsorbing and separating ethylene and propylene.
6. The method for preparing the metal organic framework material having the ability to separate ethylene and propylene by adsorption as claimed in claim 5, It is characterized in that In step 1, the usage ratio of the cobalt nitrate hexahydrate, N,N'-bis(isophthalic acid)oxalamide ligand and di(pyridin-4-yl)amine ligand is: 0.09-0.11: 0.04-0.05: 0.04-0.05; the mixed solvent is composed of 5-6 ml of N,N-dimethylformamide and 0.08-0.1 ml of concentrated nitric acid.
7. The method for preparing the metal organic framework material with ethylene and propylene adsorption separation as claimed in claim 5, It is characterized in that In step 2, the temperature of the sealed heating is 115-125° C., and the insulation time is 70 to 80 hours.
8. The method for preparing the metal organic framework material with ethylene and propylene adsorption separation as claimed in claim 5, It is characterized in that In step 4, the exchange time is 2 to 3 days.
9. The method for preparing the metal organic framework material with ethylene and propylene adsorption separation as claimed in claim 5, It is characterized in that In step 4, the vacuum heating temperature is 150-160° C. and the time is 4-6 hours.
Citation Information
Patent Citations
Cobalt metal-organic frame material and preparation method thereof
CN109134879A
Metal organic framework material with C2H2 and CH4 adsorption separation functions and preparation method thereof
CN111100149A
Metal organic framework material for efficiently separating mixed gas as well as preparation method and application thereof
CN111777769A
Metal organic framework material for adsorbing and separating ethylene and ethane as well as preparation method and application of metal organic framework material
CN113801337A
Metal organic framework material for adsorbing and separating acetylene / ethylene mixed gas and preparation method of metal organic framework material
CN115028850A