Preparation method and application of MOF on MOF heterojunction metal organic framework material rich in oxygen vacancy

By growing NiNDC and Fe BDC nanosheets in turn on the support surface, forming MOF on MOF heterojunction materials rich in oxygen defects, the problem of low catalytic performance of nickel-based MOFs is solved, and efficient redox electrocatalysis and total water decomposition are achieved. Performance, suitable for large-scale applications.

CN118930894AActive Publication Date: 2024-11-12GUANGXI NORMAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411262485.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The existing nickel-based metal organic framework materials have low catalytic performance in redox electrocatalytic reactions (OER), which limits its further promotion and application in the OER field.

Method used

NiNDC and Fe BDC nanosheets were grown sequentially on the support surface through two solvothermal reactions to form MOF on MOF heterojunction metal organic frame material NiNDC@Fe BDC, which was rich in oxygen defects, and synthesized using lattice mismatch to optimize the catalyst. structure and electronic structure.

Benefits of technology

It significantly improves the redox electrocatalytic performance and full water decomposition performance, excellent alkaline OER performance and long-term stability, simplifies the synthesis process and reduces costs, and is suitable for large-scale preparation and commercial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930894A_ABST
    Figure CN118930894A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an MOF on MOF heterojunction metal organic framework material rich in oxygen vacancy, and belongs to the technical field of electro-catalysis oxygen evolution reaction. The preparation method comprises the following steps: firstly, performing in-situ growth of a Ni NDC nanosheet on a carrier through a solution heating method, and then, growing a Fe BDC nanosheet on the surface of the Ni NDC nanosheet through the solution heating method, so as to form the Ni NDC-Fe BDC ultrathin nanosheet. According to the method, the MOF on MOF type metal organic framework can be synthesized on the premise of lattice mismatch, the synthesized Ni NDC and Fe BDC combines the advantages of multi-component material hybridization, ultrathin nanosheets, defect induction and the like, the number of active sites can be increased, and rapid transfer / redistribution of electrons in the catalytic process can be promoted. The MOF on MOF heterojunction metal organic framework has good electro-catalytic performance and excellent full water decomposition performance in an alkaline oxygen evolution reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrocatalytic oxygen evolution reaction, and in particular to a preparation method and application of an oxygen-defect-rich MOF-on-MOF heterojunction metal-organic framework material. Background Art

[0002] The process of water electrolysis includes two basic half reactions: oxygen evolution reaction (OER) and hydrogen evolution reaction (HER). Generally speaking, OER is a more complex multi-electron transfer process compared with HER (OER, 4OH - →2H 2 O+O 2 +4e - ), involving the breaking of OH bonds and the formation of O=O bonds, which has a significant impact on the overall water splitting efficiency. Metal-organic frameworks (MOFs) are a class of porous coordination polymers, known for their unique structure, huge porosity and well-defined metal coordination environment, and are widely favored in the field of OER catalysts. Among various MOFs-based electrocatalysts, nickel-based MOFs have considerable research potential because nickel resources are abundant and cost-effective compared to precious metals, and the nickel metal sites have good redox activity. However, the catalytic performance of existing nickel-based MOFs in OER is still relatively low, which limits its further promotion and application in the field of OER. Further optimization based on nickel-based MOFs to develop catalysts with excellent OER catalytic performance remains the focus of research for those skilled in the art. Summary of the invention

[0003] The purpose of the present invention is to provide a preparation method and application of an oxygen-defect-rich MOF on MOF heterojunction metal-organic framework material to solve the problems existing in the above-mentioned prior art.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] One of the technical solutions of the present invention is: a method for preparing a MOF on MOF heterojunction metal organic framework material rich in oxygen defects, by which NiNDC nanosheets (i.e., nickel-based MOF with naphthalene dicarboxylic acid as ligands) and Fe BDC nanosheets (i.e., iron-based MOF with phthalic acid as ligands) are sequentially grown on the surface of a carrier through two solvothermal reactions (i.e., solvothermal method) to obtain the MOF on MOF heterojunction metal organic framework material rich in oxygen defects.

[0006] Furthermore, the sequential growth of NiNDC nanosheets and Fe BDC nanosheets on the surface of the carrier through two solvothermal reactions specifically includes the following steps:

[0007] The carrier is added to a reaction solution 1 composed of a nickel source, naphthalene dicarboxylic acid and a solvent 1, and heated to perform a first solvothermal reaction to grow NiNDC nanosheets on the surface of the carrier; then, the carrier (Ni NDC / CP) with Ni NDC nanosheets grown on the surface is added to a reaction solution 2 composed of an iron source, phthalic acid and a solvent 2, and heated to perform a second solvothermal reaction to grow Fe BDC nanosheets on the surface of the NiNDC nanosheets to form NiNDC@Fe BDC nanosheets, thereby obtaining the oxygen-defect-rich MOF on MOF heterojunction metal-organic framework material (referred to as NiNDC@Fe BDC or Ni NDC@Fe BDC / CP, ​​CP represents the carrier).

[0008] In the present invention, the NiNDC nanosheets and Fe BDC nanosheets grown by the solvothermal method, and the Ni NDC@Fe BDC nanosheets composed of the NiNDC nanosheets and the Fe BDC nanosheets are all in the form of ultrathin nanosheets, and the thickness of the NiNDC@Fe BDC nanosheets is about 4.3 nm.

[0009] Furthermore, the nickel source is nickel chloride; the iron source is ferrous chloride; the naphthalene dicarboxylic acid is 2,6-naphthalene dicarboxylic acid (H 2 NDC); the phthalic acid is 1,4-terephthalic acid (H 2 BDC); the solvent 1 is a mixed solution of N,N-dimethylformamide (DMF) and anhydrous methanol (MeOH); the solvent 2 is a mixed solution of N,N-dimethylformamide, anhydrous ethanol (EtOH) and water; the carrier is carbon fiber paper (CP).

[0010] Furthermore, the water is ultrapure water (DI).

[0011] The carbon fiber paper has good porosity and electrical conductivity, and is resistant to high temperatures and corrosion. Its skeleton will not be destroyed under extreme conditions, and is suitable as a carrier of the MOF on MOF heterojunction metal organic framework material.

[0012] The two organic ligands play the following roles in the reaction: In the first step of the solvothermal process, H 2 NDC and Ni 2+ Coordination, participate in the synthesis of NiNDC / CP; in the subsequent secondary solvothermal process, Ni NDC / CP is immersed in the reaction solution 2, during which two important processes occur: first, NiNDC / CP acts as a carrier for in-situ growth, facilitating the growth of the catalyst; second, because Ni and Fe have similar atomic radii, ion exchange occurs during the reaction, resulting in a small amount of Fe 2+ into the Ni NDC lattice, along with Fe 2+ With H 2BDC coordinated to generate Fe BDC grew on the NiNDC surface, realizing the dynamic adaptive growth of MOFon MOF based on lattice mismatch.

[0013] In addition, H 2 NDC and H 2 BDC belongs to the carboxylic acid ligands. Selecting them as ligands for nickel and iron, respectively, is more conducive to the morphology of long sheets on the synthesis sheet in the subsequent synthesis of MOF onMOF.

[0014] Moreover, most MOFs are also prone to remodeling during the OER process, and compared with other types of ligands, the selection of H 2 NDC and H 2 The MOF onMOF obtained with BDC as a ligand is easier to reconstruct during the OER process and then quickly transformed into MOOH (M is metal) with high OER activity.

[0015] The reaction solvent plays the following roles in the reaction process: (1) It stabilizes the structure of MOF onMOF by coordinating with metal ions to form coordination bonds; (2) It regulates the polarity of the reaction solvent and controls the nucleation and growth process of MOF.

[0016] In addition, the above solvents are selected as reaction solvents in the present invention because they have the following advantages: (1) DMF, as a polar solvent, can dissolve most organic substances and many inorganic substances, and can slowly release substances such as dimethylamine during the reaction, which is beneficial to the synthesis of MOF; (2) By adding a small amount of anhydrous methanol, anhydrous ethanol and ultrapure water to DMF, the pH and polarity of the reaction solvent can be further adjusted, thereby affecting the nucleation and growth process of MOF during the reaction.

[0017] Furthermore, the nickel source is preferably nickel chloride hexahydrate (NiCl 2 6H 2 O); the iron source is preferably ferrous chloride tetrahydrate (FeCl 2 ·4H 2 O).

[0018] Furthermore, the molar ratio of the nickel source to naphthalene dicarboxylic acid in the reaction solution 1 is 4:3, and the usage ratio of naphthalene dicarboxylic acid to solvent 1 is 0.75 mmol:15 mL; the molar ratio of the iron source to phthalic acid in the reaction solution 2 is 8:15, and the usage ratio of phthalic acid to solvent 2 is 1.25 mmol:16 mL.

[0019] Furthermore, the volume ratio of N,N-dimethylformamide to anhydrous methanol in the solvent 1 is 1:1; and the volume ratio of N,N-dimethylformamide, anhydrous ethanol and water in the solvent 2 is 14:1:1.

[0020] Furthermore, the ratio of the nickel source to the carrier is 0.5 mmol: 0.5 cm 2 (Carrier surface area).

[0021] Furthermore, the reaction solution 1 is prepared by mixing a nickel source, naphthalene dicarboxylic acid and solvent 1, and subjecting the mixture to ultrasonic treatment for 15 minutes; the reaction solution 2 is prepared by mixing a nickel source, phthalic acid and solvent 2, and subjecting the mixture to ultrasonic treatment for 15 minutes.

[0022] Furthermore, the temperature of the first solvent thermal reaction is 120° C., and the time is 9 hours; the temperature of the second solvent thermal reaction is 120° C., and the time is 2 hours.

[0023] Furthermore, before the carrier is added to the reaction solution 1, a pretreatment operation of the carrier is also included. The pretreatment operation specifically includes: heating the carrier in a nitric acid solution for reaction, and then washing and drying.

[0024] The hydrophobic carbon fiber paper was transformed into hydrophilic carbon fiber paper by heating treatment in nitric acid solution, which was beneficial to the in situ growth of nanosheets.

[0025] Furthermore, the heating reaction is carried out at a temperature of 120° C. and for a time of 3 hours.

[0026] Furthermore, before heating the carrier in the nitric acid solution for reaction, the process also includes cutting the carrier (carbon fiber paper) into a size of 1 cm×2 cm.

[0027] Furthermore, the washing is specifically washing with ultrapure water and anhydrous ethanol to neutrality (pH=7).

[0028] Furthermore, after the first solvent thermal reaction and the second solvent thermal reaction are completed, washing and drying operations are also included, specifically: washing the carbon paper after the reaction with anhydrous ethanol three times, and then vacuum drying at 60° C. for 6 hours.

[0029] The present invention synthesizes oxygen-deficient MOF-on-MOF heterojunction metal-organic framework materials through two solvothermal reactions. The preparation method has the following advantages: (1) Simplified synthesis process: the two-solvothermal synthesis method is simple to operate and avoids the limitation of lattice matching strategy; (2) Simple raw materials: only two organic ligands, two metal sources and organic solvents are required, and the sources are easy to obtain;

[0030] (3) Improve product purity: The product grows on carbon fiber paper through solvent thermal reaction, which can reduce the generation of impurities.

[0031] The second technical solution of the present invention: a MOF on MOF heterojunction metal-organic framework material rich in oxygen defects prepared by the preparation method of the MOF on MOF heterojunction metal-organic framework material rich in oxygen defects as mentioned above.

[0032] The third technical solution of the present invention: an application of the above-mentioned oxygen-deficient MOF on MOF heterojunction metal-organic framework material in an electrocatalytic oxygen evolution reaction.

[0033] Furthermore, the oxygen-deficient MOF-on-MOF heterojunction metal-organic framework material is used as a catalyst for electrocatalytic oxygen evolution reaction.

[0034] Furthermore, the oxygen-deficient MOF on MOF heterojunction metal-organic framework material is used as an anode for an electrocatalytic oxygen evolution reaction in a full water splitting device.

[0035] The present invention first grows Ni NDC nanosheets in situ on a carrier by a solvothermal method, and then grows Fe BDC nanosheets on the surface of the NiNDC nanosheets by a solvothermal method to form Ni NDC@Fe BDC ultrathin nanosheets. This method can synthesize a metal organic framework of the MOF on MOF type under the premise of lattice mismatch, and the obtained metal organic framework not only has a MOF on MOF heterojunction structure, but also has a large number of oxygen vacancies. Compared with a single metal MOF, the MOF onMOF heterojunction constructed by the present invention can give full play to the advantages of the two-component MOF, and the introduced oxygen vacancies can adjust the electronic structure of the catalyst surface and optimize its hydroxyl adsorption in the alkaline OER process. The Ni NDC@Fe BDC synthesized by the present invention combines the advantages of multi-component material hybridization, ultrathin nanosheets and defect induction, which can increase the number of active sites and promote the rapid transfer / redistribution of electrons in the catalytic process. The above factors work synergistically, so that the MOF on MOF heterojunction metal organic framework has good electrocatalytic performance and excellent overall water decomposition performance in the alkaline oxygen evolution reaction.

[0036] In addition to being formed by the lattice mismatch method of the present invention, MOF onMOF materials can also be formed by lattice matching. However, most MOFs have different unit cell parameters and coordination modes. Therefore, the strategy of synthesizing MOF on MOF by lattice matching needs to consider that the two MOFs have similar lattice parameters and crystal plane matching, which has great limitations. The method of the present invention avoids the limitations of the lattice matching strategy.

[0037] The present invention discloses the following technical effects:

[0038] (1) The present invention grows oxygen-deficient MOF on MOF heterojunction metal-organic framework materials (Ni NDC@Fe BDC) on a carrier through two simple solvothermal reactions. The designed Ni NDC@Fe BDC has the characteristics of ultrathin nanosheet morphology (about 4.3nm), abundant oxygen defects and tight coupling of heterojunction interface. These characteristics effectively promote interfacial charge transfer, optimize the d-band center and enhance its adsorption capacity for oxygen-containing intermediates during the reaction process. In 1.0MKOH alkaline medium, the Ni NDC@Fe BDC material exhibits excellent OER performance and long-term stability. In addition, the material also exhibits excellent catalytic performance and stability in the overall hydrolysis reaction. These experimental results fully demonstrate that the Ni NDC@Fe BDC material prepared by the preparation method of the present invention can be regarded as an efficient electrocatalytic oxygen evolution reaction catalyst with good application prospects.

[0039] (2) The Ni NDC@Fe BDC material preparation method provided by the present invention has the advantages of simplified process, easy access to raw materials, and significantly reduced preparation time and cost. These characteristics make the material easy to prepare on a large scale and convenient for commercial production, and it has great commercial potential. More importantly, the prepared NiNDC@Fe BDC material can be directly used as an anode material in a full water splitting system, thereby greatly improving its practicality and convenience. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0041] Figure 1 X-ray powder diffraction patterns of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2.

[0042] Figure 2 Raman spectra of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2.

[0043] Figure 3 Electron paramagnetic resonance spectra of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2.

[0044] Figure 4 These are electron microscope images of Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2 of the present invention; wherein a is a scanning electron microscope image of Ni NDC / CP; and b is a scanning electron microscope image of Fe BDC / CP.

[0045] Figure 5 These are various electron microscope images of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention; wherein a is a scanning electron microscope image of Ni NDC@FeBDC / CP; bc are atomic force microscope images of Ni NDC@Fe BDC / CP; d is a transmission electron microscope image of Ni NDC@Fe BDC / CP; e is a high-resolution transmission electron microscope image of Ni NDC@Fe BDC / CP; and f is a distribution diagram of each element.

[0046] Figure 6 X-ray photoelectron energy spectra of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2; wherein a is the full XPS spectrum; b is the Ni 2p high-resolution XPS spectrum; c is the Fe2p high-resolution XPS spectrum; and de is the O1s high-resolution XPS spectrum.

[0047] Figure 7 The Ni NDC@Fe BDC / CP material prepared in Example 1 of the present invention and the Ni NDC / CP, ​​Fe BDC / CP, ​​Ni NDC-BDC / CP, ​​Ni NDC@Fe / CP and RuO prepared in Comparative Examples 1-4 and Comparative Example 6 are shown in FIG. 2 Electrochemical performance test results of / CP in 1.0 M KOH; a is the linear sweep voltammetry curve; b is the Tafel slope diagram; c is 10 mA cm -2 The overpotential and Tafel slope of the catalysts at 20 °C are compared with those of previously reported catalysts; d is the double layer capacitance (C dl ) Figure; e and f are the ECSA normalized current density at a potential of 1.47 V vs. RHE and the current density of 1 mA cm -2 The overpotential at 100 mA cm-1 is g, the OER mass activity of the catalyst is h, and the overpotential at 100 mA cm-1 is g. -2 Chronopotentiometry test of NiNDC@Fe BDC / CP.

[0048] Figure 8 The in-situ impedance diagrams of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP prepared in Comparative Example 1 in 1M KOH; a and b are Nyquist diagrams of Example 1 and Comparative Example 1 at different potentials in 1M KOH; c is Rct d and e are the Bode diagrams corresponding to the in-situ EIS tests of Example 1 and Comparative Example 1 at different potentials in 1M KOH; f is the phase angle peak of Example 1 and Comparative Example 1 at different voltages; g is the molecular orbital diagram of Example 1.

[0049] Fig. 9 In situ Raman images of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP prepared in Comparative Example 1; wherein a is an in situ Raman device image (WE, working electrode; CE, counter electrode; RE, reference electrode); b and c are the in situ Raman spectra of Example 1 and Comparative Example 1, respectively.

[0050] Fig.10 : The whole water decomposition process and results; wherein a is a schematic diagram of the whole water decomposition; b is a two-electrode system composed of the Ni NDC@Fe BDC / CP material prepared in Example 1 of the present invention and the Pt / C / CP material prepared in Comparative Example 5, and the RuO prepared in Comparative Example 6. 2 / CP materials in 1.0 M KOH; c is a comparison of the voltage of the two-electrode system composed of Ni NDC@Fe BDC / CP (This work) prepared in Example 1 of the present invention and Pt / C / CP materials prepared in Comparative Example 5 with the full water decomposition cell reported in the prior art; d is the stability test result of the two-electrode system composed of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Pt / C / CP materials prepared in Comparative Example 5.

[0051] Fig.11 Characterization of the catalyst after OER reaction; wherein, a is the HR-TEM of Ni NDC@FeBDC / CP prepared in Example 1 of the present invention after OER; b is the EPR spectra of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and NiNDC / CP prepared in Comparative Example 1 after OER.

[0052] Fig.12 The density functional theory calculation diagram of the real active species participating in the OER reaction of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP prepared in Comparative Example 1; wherein a and b are oxygen defects (O v ) of Ni(Fe)OOH; c is a schematic diagram of the bonding between the adsorbent (Ads.) and the electrocatalyst surface; d and e are the state density and partial state density diagrams; f is the Gibbs free energy diagram; g is a description of the four-electron transfer mechanism. DETAILED DESCRIPTION

[0053] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0054] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0055] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0056] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0057] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0058] Example 1

[0059] The oxygen-deficient MOF-on-MOF heterojunction metal-organic framework material (NiNDC@Fe BDC / CP) was prepared by two solvothermal reactions. The steps are as follows:

[0060] (1) Pretreatment of carrier: Cut carbon fiber paper into 1×2 cm 2 The size was then heated in a nitric acid solution (concentration of 8 mol / L) at 120°C for 3 hours, followed by ultrasonic washing with ultrapure water and anhydrous ethanol in turn until the pH of the washing solution was 7, and then naturally dried for use.

[0061] (2) Prepare reaction solution 1: 1 mmol NiCl 2 6H2 O and 0.75 mmol H 2 NDC (2,6-naphthalene dicarboxylic acid) was dissolved in a mixed solution consisting of 7.5 mL DMF and 7.5 mL MeOH, and ultrasonicated for 15 minutes to obtain a reaction solution 1.

[0062] (3) First solvothermal reaction: The carbon fiber paper treated in step (1) is placed in the reaction solution 1 prepared in step (2), and the reaction is carried out in an oven at 120° C. for 9 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60° C. for 6 hours to complete the growth of Ni NDC nanosheets on the surface of the carbon fiber paper.

[0063] (4) Prepare reaction solution 2: 0.4 mmol FeCl 2 ·4H 2 O and 1.25 mmol H 2 BDC (1,4-terephthalic acid) was dissolved in a mixed solution consisting of 14 mL DMF, 1 mL EtOH and 1 mL DI, and ultrasonicated for 15 minutes to obtain a reaction solution 2.

[0064] (5) Second solvothermal reaction: The carbon fiber paper with Ni NDC nanosheets grown on the surface prepared in step (3) is placed in the reaction solution 2 prepared in step (4), and the reaction is carried out at 120° C. in an oven for 2 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60° C. for 6 hours to complete the growth of Fe BDC nanosheets on the surface of NiNDC nanosheets to form NiNDC@Fe BDC ultrathin nanosheets, thereby obtaining a MOF on MOF heterojunction metal organic framework material rich in oxygen defects. The final product is recorded as Ni NDC@Fe BDC / CP.

[0065] Comparative Example 1

[0066] The NiNDC / CP material is prepared by a one-step solvothermal reaction, and the steps are as follows:

[0067] (1) Pretreatment of carrier: Cut carbon fiber paper into 1×2 cm 2 The size was then heated in a nitric acid solution (concentration of 8 mol / L) at 120°C for 3 hours, followed by ultrasonic washing with ultrapure water and anhydrous ethanol in turn until the pH of the washing solution was 7, and then naturally dried for use.

[0068] (2) Prepare reaction solution 1: 1 mmol NiCl 2 6H 2 O and 0.75 mmol H 2NDC was dissolved in a mixed solution consisting of 7.5 mL of DMF and 7.5 mL of MeOH and subjected to ultrasonic treatment for 15 minutes to obtain a reaction solution 1.

[0069] (3) One-step solvothermal reaction: The carbon fiber paper treated in step (1) is placed in the reaction solution 1 prepared in step (2), and the reaction is carried out in an oven at 120°C for 9 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60°C for 6 hours to complete the growth of Ni NDC nanosheets on the surface of the carbon fiber paper to obtain Ni NDC / CP material.

[0070] Comparative Example 2

[0071] The Fe BDC / CP material was prepared by a one-step solvothermal reaction, and the steps are as follows:

[0072] (1) Pretreatment of carrier: Cut carbon fiber paper into 1×2 cm 2 The size was then heated in a nitric acid solution (concentration of 8 mol / L) at 120°C for 3 hours, followed by ultrasonic washing with ultrapure water and anhydrous ethanol in turn until the pH of the washing solution was 7, and then naturally dried for use.

[0073] (2) Prepare reaction solution 2: 0.4 mmol FeCl 2 ·4H 2 O and 1.25 mmol H 2 BDC was dissolved in a mixed solution consisting of 14 mL DMF, 1 mL EtOH and 1 mL DI, and ultrasonicated for 15 minutes to obtain reaction solution 2.

[0074] (3) One-step solvothermal reaction: The carbon fiber paper treated in step (1) is placed in the reaction solution 2 prepared in step (2), and the reaction is carried out in an oven at 120°C for 2 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60°C for 6 hours to complete the growth of Fe BDC nanosheets on the surface of the carbon fiber paper to obtain Fe BDC / CP material.

[0075] Comparative Example 3

[0076] The Ni NDC-BDC / CP material was prepared by two solvothermal reactions, and the steps are as follows:

[0077] (1) Pretreatment of carrier: Cut carbon fiber paper into 1×2 cm 2 The size was then heated in a nitric acid solution (concentration of 8 mol / L) at 120°C for 3 hours, followed by ultrasonic washing with ultrapure water and anhydrous ethanol in turn until the pH of the washing solution was 7, and then naturally dried for use.

[0078] (2) Prepare reaction solution 1: 1 mmol NiCl 2 6H 2 O and 0.75 mmol H 2 NDC was dissolved in a mixed solution consisting of 7.5 mL of DMF and 7.5 mL of MeOH and subjected to ultrasonic treatment for 15 minutes to obtain a reaction solution 1.

[0079] (3) First solvothermal reaction: The carbon fiber paper treated in step (1) is placed in the reaction solution 1 prepared in step (2), and the reaction is carried out in an oven at 120° C. for 9 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60° C. for 6 hours to complete the growth of Ni NDC nanosheets on the surface of the carbon fiber paper.

[0080] (4) Prepare reaction solution 2: 1.25 mmol H 2 BDC was dissolved in a mixed solution consisting of 14 mL DMF, 1 mL EtOH and 1 mL DI and sonicated for 15 min to obtain reaction solution 2.

[0081] (5) Second solvothermal reaction: The carbon fiber paper with Ni NDC nanosheets grown on the surface obtained in step (3) is placed in the reaction solution 2 prepared in step (4), and the reaction is carried out in an oven at 120° C. for 2 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60° C. for 6 hours to obtain a NiNDC-BDC / CP material.

[0082] Comparative Example 4

[0083] The NiNDC@Fe / CP material was prepared by two solvothermal reactions, and the steps are as follows:

[0084] (1) Pretreatment of carrier: Cut carbon fiber paper into 1×2 cm 2 The size was then heated in a nitric acid solution (concentration of 8 mol / L) at 120°C for 3 hours, followed by ultrasonic washing with ultrapure water and anhydrous ethanol in turn until the pH of the washing solution was 7, and then naturally dried for use.

[0085] (2) Prepare reaction solution 1: 1 mmol NiCl 2 6H 2 O and 0.75 mmol H 2 NDC was dissolved in a mixed solution consisting of 7.5 mL of DMF and 7.5 mL of MeOH and subjected to ultrasonic treatment for 15 minutes to obtain a reaction solution 1.

[0086] (3) First solvothermal reaction: The carbon fiber paper treated in step (1) is placed in the reaction solution 1 prepared in step (2), and the reaction is carried out in an oven at 120° C. for 9 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60° C. for 6 hours to complete the growth of Ni NDC nanosheets on the surface of the carbon fiber paper.

[0087] (4) Prepare reaction solution 2: 0.4 mmol FeCl 2 ·4H 2 O was dissolved in a mixed solution consisting of 14 mL DMF, 1 mL EtOH and 1 mL DI and sonicated for 15 min to obtain reaction solution 2.

[0088] (5) Second solvothermal reaction: The carbon fiber paper with Ni NDC nanosheets grown on the surface obtained in step (3) is placed in the reaction solution 2 prepared in step (4), and the reaction is carried out in an oven at 120° C. for 2 hours. After the reaction is completed, the carbon fiber paper is naturally cooled, and the carbon fiber paper after the reaction is rinsed three times with anhydrous ethanol, and then vacuum dried at 60° C. for 6 hours to obtain NiNDC@Fe / CP material.

[0089] Comparative Example 5

[0090] Preparation of Pt / C / CP electrode materials

[0091] 2 mg Pt / C (commercially available, Pt mass fraction 20%) was weighed and added to a mixed solution of 125 μL ultrapure water, 125 μL anhydrous ethanol and 25 μL Nafion solution, and ultrasonically dissolved for 30 minutes. Then, the ultrasonically homogenized Pt / C slurry was dropped on a 0.5 cm 2 The carbon fiber paper was placed on the plate and dried at room temperature for later use.

[0092] Comparative Example 6

[0093] RuO 2 Preparation of / CP electrode materials

[0094] Weigh 2 mg RuO 2 (commercially available) was added to a mixed solution of 125 μL ultrapure water, 125 μL anhydrous ethanol and 25 μL Nafion solution, and ultrasonically dissolved for 30 minutes. 2 The slurry was dropped at 0.5 cm 2 The carbon fiber paper was placed on the plate and dried at room temperature for later use.

[0095] Effect verification

[0096] 1. Physical structure and morphology characterization

[0097] (1) Figure 1 The X-ray powder diffraction patterns of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2 are shown in FIG. Figure 1 It can be seen that for Ni NDC@Fe BDC / CP, ​​the peaks around 7.4°, 14.8°, and 15.1° correspond to the (001), (012), and (011) crystal planes of Ni NDC, respectively. The peaks at about 8.8° and 9.4° come from the (048) and (139) crystal planes of Fe BDC. These results confirm the synthesis of MOF on MOF heterostructures. Figure 2 The Raman spectra of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2 are shown. Figure 2 It can be seen that all materials are between 1100-1750cm -1 The characteristic peaks of organic ligands are shown in the range of 2.47 nm, which means the successful preparation of MOF. For Ni NDC@Fe BDC / CP, ​​in addition to the original H 2 In addition to the NDC characteristic peak, 875cm -1 The new peak at 2 The CH vibration of the benzene ring in BDC indicates that H 2 NDC and H 2 Two organic ligands coexist in BDC. At the same time, compared with Ni NDC / CP, ​​the peak of Ni-O bond vibration in NiNDC@Fe BDC / CP is slightly blue-shifted ( Figure 2 Medium 520cm -1 This may be caused by the phonon confinement effect induced by surface oxygen vacancies, and also reveals the strengthening of Ni-O bonds in Ni NDC@Fe BDC / CP. Figure 3 Electron paramagnetic resonance spectra of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2. Figure 3 It can be seen that compared with Ni NDC / CP and Fe BDC / CP, ​​Ni NDC@Fe BDC / CP shows abundant oxygen vacancies and produces a stronger EPR signal at g = 2.003, indicating that there are more oxygen defects at the lattice mismatch growth interface.

[0098] (2) Figure 4 The scanning electron microscope images of Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2 of the present invention are shown in Figure 1; wherein a is the Ni NDC / CP of Comparative Example 1; and b is the Fe BDC / CP of Comparative Example 2. Figure 4It can be seen that the Ni NDC / CP precursor presents a smooth ultrathin nanosheet morphology. If the Ni NDC / CP precursor is not used, the individual Fe BDC nanoparticles will be severely agglomerated when grown on carbon paper. Figure 5 Various electron microscope images of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention; wherein, a is a scanning electron microscope image of Ni NDC@Fe BDC / CP, ​​it can be found that the ultra-thin nanosheet morphology can still be maintained, but due to the introduction of Fe BDC, the surface of the nanosheet becomes slightly rough, which may be beneficial to the mass transfer process in electrocatalysis. d and e are high-resolution transmission electron microscope images (HR-TEM) of NiNDC@Fe BDC / CP, ​​the lattice spacing at 0.99 and 0.93nm corresponds to the Fe BDC (048) and (139) crystal planes, and the lattice spacing at 1.18 and 0.58nm corresponds to the NiNDC (001) and (011) crystal planes, which further indicates the successful synthesis of NiNDC@Fe BDC / CP. It is worth noting that in the HR-TEM image of Ni NDC@Fe BDC / CP, ​​it is found that some lattice spacings have a large number of dislocations and distortions (as shown in the dotted box in d), indicating that there are a large number of defects in the prepared catalyst. These lattice defects may expose more active sites, thereby improving the efficiency of OER. f is the distribution diagram of each element (EDS), indicating that the Ni, Fe and O elements in Ni NDC@Fe BDC / CP are evenly distributed, indicating that H 2 The introduction of BDC ligands does not cause heterogeneous coordination between the ligand functional groups and metal ions. b and c are atomic force microscopy images and the corresponding height profiles, confirming that the average thickness of Ni NDC@Fe BDC / CP is about 4.3 nm.

[0099] (5) Figure 6 X-ray photoelectron spectra of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP and Fe BDC / CP prepared in Comparative Examples 1-2; wherein, a is the full XPS spectrum; b is the Ni 2p high-resolution XPS spectrum; c is the Fe2p high-resolution XPS spectrum; and de is the O1s high-resolution XPS spectrum. The full spectrum of Ni NDC@Fe BDC / CP shows the coexistence of O, Ni, and Fe, which is completely consistent with the previous EDS spectrum results. The Ni 2p spectrum supports the coexistence of Ni 2+ The presence of oxidation states, the characteristic peaks at 856 and 873.1 eV are attributed to Ni 2+ 2p 3 / 2 and Ni 2+ 2p 1 / 2Compared with pure Ni NDC / CP, ​​the Ni 2p peak of Ni NDC@Fe BDC / CP shifts to a lower binding energy, indicating that the local electronic environment of Ni has changed. As for the Fe 2p spectrum, the peaks at binding energies of 711.8 and 725.9 eV correspond to Fe 3+ , while the peaks at 710.4 and 723.4 eV belong to Fe 2+ Obviously, the Fe in Ni NDC@Fe BDC / CP 3+ / Fe 2+ The ratio (1.92) is larger than that in Fe BDC / CP (1.48), which indicates that the Fe in the MOF-on-MOF heterojunction is bounded by the bridging oxygen of the organic ligands. 3+ Similarly, in the O1s spectrum, the peaks near 529.8, 531.2, and 532.5 eV are defined as metal oxygen bonds (MO), oxygen vacancy defects (Ov), and absorbed water (H 2 O ads ). It is worth noting that due to the absence of oxygen defects in single metal MOFs, the O 1s peak is fitted to CO / C=O, MO and H 2 O ads In summary, these results indicate that the Ni-Fe synergistic effect and oxygen defects exist in NiNDC@Fe BDC / CP, ​​which provide the necessary conditions for its efficient OER catalytic performance.

[0100] 2. Electrochemical test

[0101] Test method: All electrochemical measurements were performed using a multi-channel electrochemical workstation (Bio-logic VMP3, France) with a typical three-electrode system in 1.0 M KOH solution. The prepared catalyst material, carbon rod, and Hg / HgO electrode were used as the working electrode, counter electrode, and reference electrode, respectively. The current was 5 mV s in the range of 1.1-1.8 V (vs. RHE). -1 Linear sweep voltammetry (LSV) was performed at a scan rate of 1.5 Å, and all polarization curves were iR (95%) corrected. The measured potentials were converted to the RHE scale using the Nernst equation:

[0102] E RHE =E SCE +0.241+0.059pH-iR

[0103] Test results:

[0104] (1) Figure 7The Ni NDC@Fe BDC / CP material prepared in Example 1 of the present invention and the Ni NDC / CP, ​​Fe BDC / CP, ​​Ni NDC-BDC / CP, ​​Ni NDC@Fe / CP and RuO prepared in Comparative Examples 1-4 and Comparative Example 6 are shown in FIG. 2 Electrochemical performance test results of / CP in 1.0 M KOH; a is the linear sweep voltammetry curve; b is the Tafel slope diagram; c is 10 mA cm -2 The overpotential and Tafel slope of the catalysts reported previously are compared (This work represents the NiNDC@Fe BDC / CP material prepared in Example 1 of the present invention); d is the double layer capacitance (C dl ) Figure; e and f are the ECSA normalized current density at a potential of 1.47 V vs. RHE and the current density of 1 mA cm -2 ; g is the OER mass activity of the catalyst; h is 100 mA cm -2 Figure a shows that the optimized Ni NDC@Fe BDC / CP has a current density of 10 mA cm -2 The overpotential is 192 mV, which is lower than Ni NDC@Fe / CP (214 mV), Ni NDC@BDC / CP (280 mV), Ni NDC / CP (269 mV), and RuO 2 / CP (298mV) and Fe BDC / CP (370mV). At 100mAcm -2 At a current density of 2.5 Å, the overpotential of Ni NDC@FeBDC / CP is 239 mV, which is also competitive compared with other samples. The Tafel slope value of Ni NDC@Fe BDC / CP in Figure b is 38.8 mV dec. -1 , lower than Ni NDC@Fe / CP (46.9mV dec -1 )、Ni NDC@BDC / CP(74.1mV dec -1 )、Ni NDC / CP(105.5mV dec -1 ),RuO 2 / CP(77.4mV dec -1 ) and Fe BDC / CP (64.6mV dec -1), indicating that Ni NDC@Fe BDC / CP has faster electrocatalytic kinetics. c is the overpotential and Tafel slope of Ni NDC@Fe NDC / CP (This work) and the catalysts reported in the prior art [S-NiFe / NFF (10.1016 / j.jelechem.2023.117365), NiFe-MOF-5 (10.1039 / D2DT00127F), NiFe-MOF-74 (10.1039 / C8CC03112F), CTGU-10c2 (10.1002 / anie.201813634), Mn-MOF / CuO (10.1016 / j.fuel.2023.127638), Ni 0.75 Fe 0.25 Se 2 @NF(6H)(10.1016 / j.apsusc.2019.05.220)、Fe 2 O 3 @Ni-MOF-74(10.1021 / acs.inorgchem.9b01301), GO@Ce MOF(10.1002 / app.51571), MnSe@MWCNT(10.1039 / D1TA09864K), FeNiCo@NC / NF-600(10.1016 / j.jpowsour.2020.228866)]. The electrochemically active surface area (ECSA) is an important criterion that directly reflects the surface area activity: the larger the ECSA value, the more active sites it means. ECSA and double layer capacitance (C dl ) can be calculated by cyclic voltammetry tests in the non-Faraday range at different scan rates. As shown in Figure d, Ni NDC@Fe BDC / CP shows a larger C dl (7.4mFcm -2 ), which indicates that the catalyst has a high specific surface area. Next, the ECSA-normalized LSV curves were calculated to understand the intrinsic activity of different catalysts. As shown in Figure ef, the ECSA-normalized LSV curves show that the intrinsic activity of NiNDC@Fe BDC / CP has been substantially improved. At a potential of 1.47 V (vs. RHE), the ECSA-normalized current density of Ni NDC@Fe BDC / CP is estimated to be 0.56 mA cm -2 , which is higher than other catalysts. In addition, 1mA cm -2The overpotential of Ni NDC@Fe BDC / CP is only 250 mV, which is significantly lower than that of the original Ni NDC / CP (290 mV). It is worth noting that the turnover frequency (TOF) is also an important parameter for comparing the intrinsic activity of the catalyst. The TOF value of Ni NDC@Fe BDC / CP is higher than that of other comparison samples, which strongly proves that NiNDC@Fe BDC / CP has more accessible active sites and higher intrinsic activity (Figure g). In addition to the electrocatalytic activity, the stability of the catalyst is also crucial for practical applications. The long-term stability of NiNDC@Fe BDC / CP was verified by constant current testing in 1.0 M KOH. -2 At a current density of 2.5 Å, the voltage of Ni NDC@Fe BDC / CP showed little significant change within 100 h (Figure h), which indicates its excellent stability.

[0105] Figure 8 The in-situ impedance diagrams of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP prepared in Comparative Example 1 in 1M KOH; a and b are Nyquist diagrams of Example 1 and Comparative Example 1 at different potentials in 1M KOH; c is R ct d and e are the Bode diagrams corresponding to the in-situ EIS test of Example 1 and Comparative Example 1 at different potentials in 1M KOH; f is the phase angle peak of Example 1 and Comparative Example 1 at different voltages; g is the molecular orbital diagram of Example 1. It can be clearly seen from the AC impedance spectra in a and b that NiNDC@Fe BDC / CP clearly exhibits a lower charge transfer resistance within the applied potential range, which indicates that the strong heterojunction coupling effect in NiNDC@Fe BDC / CP can significantly promote interfacial charge transfer and surface activation of the catalyst. R ct It can be used to describe the adsorption resistance of oxygen-containing active intermediates, R ct The changing trend of R reveals the OH* change process on the catalyst surface. ct According to the fitting results, the R of NiNDC@Fe BDC / CP under the applied potential ct The values ​​are lower than those of NiNDC / CP, ​​which indicates that it has faster adsorption kinetics for oxygen-containing intermediates in the OER process. From the df, it can be seen that the phase peak of Ni NDC@Fe BDC / CP in the low-frequency region shows a lower phase angle at each applied potential, which indicates that the deprotonation rate of the intermediates in the OER process is faster and consistent with the C dl This is consistent with the results of ECSA normalized LSV. This enhanced intrinsic activity can be explained by crystal field theory. As shown in g, Ni in Ni NDC2+ t 2g The orbital is fully occupied, resulting in Ni 2+ With bridge O 2- After the introduction of Fe BDC, the 3+ Coordinated H 2 BDC organic ligand is a strong field ligand, and its d orbital splitting energy is higher than the pairing energy, resulting in Fe 3+ The valence electron configuration is t in a low spin state. 2g 5 e g 0 Compared with Ni NDC, there are abundant oxygen defects on the heterojunction interface of NiNDC@Fe BDC, which not only promotes the delocalization of electrons on the Fe-O bond, but also causes part of the electrons on the Ni-O bond to migrate to the Ni active center, thereby optimizing the electronic structure and catalytic reaction activity of Ni NDC@FeBDC in this complex way. When electrons are transferred from Fe to Ni, the electrons in the Fe 3d orbital will rearrange to produce high-spin Fe species, which is beneficial to OER. In short, this electron transfer between NiFe optimizes the catalyst t 2g The electron distribution on the orbit is more conducive to the adsorption of active intermediates.

[0106] Fig. 9 The in-situ Raman images of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP prepared in Comparative Example 1; a is the in-situ Raman device image (WE, working electrode; CE, counter electrode; RE, reference electrode); b and c are the in-situ Raman spectra of Example 1 and Comparative Example 1, respectively. Obviously, as the applied potential gradually increases, the characteristic peaks of the original MOF gradually disappear, and are replaced by Ni(Fe)OOH E g Bending vibration and A 1g Characteristic peaks of stretching vibration. Compared with Ni NDC / CP, ​​Ni NDC@Fe BDC / CP can generate MOOH (M represents metal) phase at a lower potential, indicating that constructing defective heterojunctions on a single Ni MOF can improve the intrinsic activity of Ni NDC and accelerate the conversion of precatalysts to the real active species Ni(Fe)OOH participating in the reaction.

[0107] (2) Fig.101 is a schematic diagram of the whole water decomposition process and results; wherein a is a schematic diagram of the whole water decomposition (wherein Pt / C represents Pt / C / CP prepared in Comparative Example 5, and Ni NDC@Fe BDC represents Ni NDC@Fe BDC / CP prepared in Example 1); b is a two-electrode system composed of the Ni NDC@Fe BDC / CP material prepared in Example 1 of the present invention and the Pt / C / CP material prepared in Comparative Example 5, and the RuO prepared in Comparative Example 6. 2 Polarization curves of the two-electrode system composed of / CP materials in 1.0MKOH. From b, we can see that Ni NDC@Fe BDC / CP (+) ||Pt / C / CP (-) Only 1.43 and 1.54 V battery voltages are required to achieve 10 and 100 mA cm -2 The current density is better than that of RuO 2 / CP (+) ||Pt / C / CP (-) The performance of the Ni NDC@Fe BDC / CP material prepared in the present invention shows that the Ni NDC@Fe BDC / CP material prepared in the present invention has excellent full water splitting performance. c is a two-electrode system composed of the NiNDC@Fe BDC / CP prepared in Example 1 of the present invention (This work) and the Pt / C / CP material prepared in Comparative Example 5 and the full water splitting battery reported in the prior art [NFN MOF / NF (10.1002 / aenm.201801065), CoNiRu / NT (10.1002 / adma.202107488), Co-NC@Ni 2 Fe-LDH(10.1002 / smll.202107739), Ni-250-2@NF(10.1039 / D2TA09369C), IrO 2 @Ir MOF(10.1039 / D0TA09168E), Ir@Ni NDC(10.1002 / ange.202302220), Ce@NiFe MOF(10.1021 / acs.inorgchem.2c04261), Ru-NiFe-P / Ni(10.1016 / j.apcatb.2019.118324), Mo-RuCoO x (10.1002 / adfm.202303073), FeNiMo (10.1021 / acsmaterialslett.4c00930), NiCo 2 O 4d is the stability test result of the two-electrode system composed of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Pt / C / CP prepared in Comparative Example 5. It can be seen from d that NiNDC@Fe BDC / CP (+) ||Pt / C / CP (-) At 100mAcm -2 After continuous operation for 50 h at a constant current density, there was no obvious potential decay, demonstrating an impressive overall water splitting stability.

[0108] 3. Density functional theory calculations

[0109] Fig.11 : Characterization of the catalyst after OER reaction, where a is the HR-TEM of Ni NDC@FeBDC / CP prepared in Example 1 of the present invention after OER, and b is the EPR spectrum of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and NiNDC / CP prepared in Comparative Example 1 after OER. It can be seen that Ni NDC / CP still has no oxygen defects after OER test, on the contrary, NiNDC@Fe BDC / CP has abundant oxygen defects, which illustrates the stability of oxygen defects in Ni NDC@Fe BDC / CP heterojunction. Combined with in situ Raman ( Fig. 9 ) and EPR( Fig.11 From the test results in (b), it can be inferred that Ni NDC@Fe BDC actually acts as a pre-catalyst in the OER reaction. It undergoes reconstruction during the OER process, and the generated Ni(Fe)OOH with rich oxygen defects is the real active species participating in the reaction. Correspondingly, Ni NDC is reconstructed into defect-free NiOOH in electrochemistry to participate in the OER.

[0110] Fig.12 The density functional theory calculation diagram of the real active species participating in the OER reaction of Ni NDC@Fe BDC / CP prepared in Example 1 of the present invention and Ni NDC / CP prepared in Comparative Example 1; wherein a and b are oxygen defects (O v ) of Ni(Fe)OOH; c is a schematic diagram of the bonding between the adsorbent (Ads.) and the electrocatalyst surface; d and e are the state density and partial state density diagrams; f is the Gibbs free energy diagram; g is a diagram describing the four-electron transfer mechanism. b shows that there is a strong electronic interaction between Ni, Fe and O, and the v The charge accumulation around O atoms in Ni(Fe)OOH indicates that electrons are transferred from Ni / Fe to O atoms, which is consistent with the XPS results. The calculated density of states in d shows that the Ov The increased state density of Ni(Fe)OOH near the Fermi level means that more charge carriers are directly involved in the catalytic reaction, which significantly improves the OER performance of the catalyst. v Compared with NiOOH (-1.25 eV), O v The d-band center (εd) (-1.23 eV) of Ni(Fe)OOH is closer to the Fermi level, which is beneficial for exposing active sites and adsorbing active intermediates ( Fig.12 According to the d-band center theory, the electronic interaction between the adsorbent and the electrocatalyst can be explained as the coupling between the valence state of the adsorbent and the d-band center of the transition metal, resulting in the formation of split bonding and anti-bonding states ( Fig.12 (c) The bonding states below the Fermi level are usually filled, while the antibonding states of NiOOH rise after the introduction of iron doping and oxygen defects, resulting in an increase in the adsorption capacity of the reaction intermediates during the OER process. According to the widely accepted AEM mechanism of the alkaline OER process and previous experimental results, the best model of the Ni(Fe)OOH intermediate is explained in g, where the Ni site is regarded as the adsorption site. As shown in f, the conversion of *O to *OOH is O v Ni(Fe)OOH and O-free v NiOOH is the rate-determining step during the OER. v The △G3 (1.54 eV) of Ni(Fe)OOH is lower than that of Ni(Fe)OOH without O v The △G3 (1.88 eV) of NiOOH further proves theoretically that the former has better OER kinetics.

[0111] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a MOF-on-MOF heterojunction metal-organic framework material rich in oxygen defects, characterized in that: Through two solvothermal reactions, NiNDC nanosheets and Fe BDC nanosheets are sequentially grown on the surface of the carrier to obtain the MOF on MOF heterojunction metal organic framework material rich in oxygen defects.

2. The method for preparing the oxygen-deficient MOF on MOF heterojunction metal-organic framework material according to claim 1, characterized in that: The method of sequentially growing NiNDC nanosheets and Fe BDC nanosheets on the surface of the carrier through two solvothermal reactions specifically includes the following steps: The carrier is added to a reaction solution 1 composed of a nickel source, naphthalene dicarboxylic acid and a solvent 1, and heated to perform a first solvothermal reaction to grow NiNDC nanosheets on the surface of the carrier; then, the carrier with the NiNDC nanosheets grown on the surface is added to a reaction solution 2 composed of an iron source, phthalic acid and a solvent 2, and heated to perform a second solvothermal reaction to grow Fe BDC nanosheets on the surface of the Ni NDC nanosheets to form NiNDC@Fe BDC nanosheets, thereby obtaining the oxygen-defect-rich MOF onMOF heterojunction metal-organic framework material.

3. The method for preparing the oxygen-deficient MOF-on-MOF heterojunction metal-organic framework material according to claim 2, characterized in that: The nickel source is nickel chloride; the iron source is ferrous chloride; the naphthalene dicarboxylic acid is 2,6-naphthalene dicarboxylic acid; the phthalic acid is 1,4-terephthalic acid; the solvent 1 is a mixed solution of N,N-dimethylformamide and anhydrous methanol; the solvent 2 is a mixed solution of N,N-dimethylformamide, anhydrous ethanol and water; and the carrier is carbon fiber paper.

4. The method for preparing the oxygen-deficient MOF on MOF heterojunction metal-organic framework material according to claim 2, characterized in that: The molar ratio of the nickel source to naphthalene dicarboxylic acid in the reaction solution 1 is 4:3, and the usage ratio of naphthalene dicarboxylic acid to solvent 1 is 0.75 mmol:15 mL; the molar ratio of the iron source to phthalic acid in the reaction solution 2 is 8:25, and the usage ratio of phthalic acid to solvent 2 is 1.25 mmol:16 mL.

5. The method for preparing the oxygen-deficient MOF on MOF heterojunction metal-organic framework material according to claim 3, characterized in that: The volume ratio of N,N-dimethylformamide to anhydrous methanol in the solvent 1 is 1:1; the volume ratio of N,N-dimethylformamide, anhydrous ethanol and water in the solvent 2 is 14:1:

1.

6. The method for preparing the oxygen-deficient MOF-on-MOF heterojunction metal-organic framework material according to claim 2, characterized in that: The temperature of the first solvent thermal reaction was 120° C. and the time was 9 hours; the temperature of the second solvent thermal reaction was 120° C. and the time was 2 hours.

7. The method for preparing the oxygen-deficient MOF-on-MOF heterojunction metal-organic framework material according to claim 2, characterized in that: Before the carrier is added into the reaction solution 1, a pretreatment operation of the carrier is also included. The pretreatment operation specifically includes: heating the carrier in a nitric acid solution for reaction, and then washing and drying.

8. The method for preparing the oxygen-deficient MOF-on-MOF heterojunction metal-organic framework material according to claim 7, characterized in that: The heating reaction was carried out at a temperature of 120° C. and for 3 hours.

9. A MOF on MOF heterojunction metal-organic framework material rich in oxygen defects prepared by the method for preparing a MOF on MOF heterojunction metal-organic framework material rich in oxygen defects as described in any one of claims 1 to 8.

10. Use of the oxygen-deficient MOF-on-MOF heterojunction metal-organic framework material according to claim 9 in an electrocatalytic oxygen evolution reaction.

Citation Information

Patent Citations

  • Ultrathin Ni-Fe-MOF nanosheet, preparation method and application thereof

    CN109267093A

  • Fe-doped Ni-MOF nanosheet as well as preparation method and application thereof

    CN113563596A

  • Preparation method of iron-based metal organic framework composite material with MOF-On-MOF framework, obtained product and application

    CN114409914A

  • MOF-on-MOF composite membrane material and preparation method thereof

    CN115627003A

  • Synthesis method of MOF-on-MOF material and application of chlorpyrifos detection

    CN116284810A