Fluorodiene modified radiation vulcanization cross-linked perfluoroether elastomer composition and preparation method thereof

After devolatilization and passivation treatment of liquid or supercritical fluid, combined with radiation vulcanization cross-linking technology, the poor performance and environmental problems of perfluoroether elastomer during secondary vulcanization are solved, forming permanent with excellent mechanical properties and low compression Deformed elastomer, suitable for high-clean semiconductor processes.

CN118930909APending Publication Date: 2024-11-12SHANGHAI MORISEAL NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411087659.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the secondary vulcanization process, existing perfluoroelastomers have problems such as poor product performance, gas release problems, unfriendly environment and low productivity, which affects their stability and application performance in high temperature and oxidation environments.

Method used

Fluorodiolefin-modified perfluoroether elastomer is devolatilized and passivated by liquid or supercritical fluid, and then through radiation vulcanization cross-linking technology, a grid structure is formed to improve mechanical properties and storage stability, and at high temperatures Vulcanization shaping is carried out in a short time.

Benefits of technology

The excellent processability and storage stability of perfluoroelastomer are achieved, the risk of discoloration in high temperature and oxidation environments is reduced, mechanical properties and low compression permanent deformation performance are improved, making it suitable for highly clean semiconductor processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930909A_ABST
    Figure CN118930909A_ABST
Patent Text Reader

Abstract

The invention provides a fluoroalkadiene modified radiation vulcanization cross-linked perfluoroether elastomer composition and a preparation method thereof, and belongs to the technical field of fluoroelastomers, and the preparation method specifically comprises the following steps: S1, using a liquid or a supercritical fluid to devolatilize a fluoroalkadiene modified perfluoroether elastomer; s2, carrying out passivation treatment on the devolatilized perfluoroether elastomer under a swelling condition, and removing a passivation medium; s3, deionized water is used for washing the passivated perfluoroether elastomer, vacuum drying is carried out after dehydration, and the devolatilized and passivated perfluoroether elastomer is obtained; s4, mixing and thin-passing the devolatilized and passivated perfluoroether elastomer, adding a vulcanizing agent and a filling agent, and carrying out compression molding; and S5, carrying out radiation vulcanization on the compression-molded perfluoroether elastomer, and carrying out short-time high-temperature vulcanization shaping to obtain the perfluoroether elastomer composition. The perfluoroether elastomer treated by the invention has excellent processability and storage stability, and is not easy to discolor when being in contact with high-temperature and oxidation environments in subsequent processing and using processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluoroelastomers, and in particular to a fluorodiene-modified radiation-vulcanized cross-linked perfluoroether elastomer composition and a preparation method thereof. Background Art

[0002] Perfluoroether elastomer composition is a heat-resistant elastomer, usually used at high temperatures, so secondary vulcanization is a necessary step in the production process of its products. The main purpose of secondary vulcanization is to complete the reaction of the unreacted cross-linking groups remaining after the first compression molding vulcanization; at the same time, remove the cross-linking reaction residues produced during the first vulcanization process.

[0003] However, secondary vulcanization has the following effects on the performance of the finished product: 1) Improve the mechanical properties and compression set properties of products; 2) If the gas release during the secondary vulcanization process can be effectively controlled, the gas generated during the use of the product can be reduced, that is, the shrinkage rate of the product can be reduced; if it is not well controlled, the defective rate of the product will increase, which is manifested in the formation of pores on the surface of the product and the failure of internal gas to release, resulting in a decrease in the local strength of the product.

[0004] 3) The gas release during high-temperature vulcanization is not environmentally friendly. In addition, the secondary vulcanization time is as long as 20 hours, and the productivity is low.

[0005] Therefore, there is an urgent need for a preparation method that can quickly produce a perfluoroether elastomer composition. Summary of the invention

[0006] Therefore, in order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a fluorodiene modified radiation vulcanized cross-linked perfluoroether elastomer composition and a preparation method thereof, wherein the perfluoroether elastomer composition has excellent processability and storage stability, and is not easy to change color when exposed to high temperature and oxidative environment during subsequent processing and use.

[0007] In order to achieve the above-mentioned object, the present invention provides a method for preparing a fluorodiene-modified radiation-cured cross-linked perfluoroether elastomer composition, comprising: S1, using a liquid or a supercritical fluid to devolatilize a fluorodiene-modified perfluoroether elastomer; the fluorodiene-modified perfluoroether elastomer is obtained by emulsion polymerization of 43-68 parts by mass of tetrafluoroethylene, 30-55 parts of perfluoroalkyl vinyl ether, 0.05-0.8 parts of iodine-containing chain transfer agent, 0.3-0.5 parts of peroxide initiator and 1-2 parts of non-conjugated fluorodiene as a vulcanization point monomer; and the hyperbranched perfluoroether elastomer is prepared by emulsion polymerization of 43-68 parts by mass of tetrafluoroethylene, 30-55 parts of perfluoroalkyl vinyl ether, 0.05-0.8 parts of iodine-containing chain transfer agent, 0.3-0.5 parts of peroxide initiator and 1-2 parts of non-conjugated fluorodiene as a vulcanization point monomer. S1, co-precipitation and condensation of the body emulsion and the PFA emulsion, and washing to obtain a fluorodiene-modified perfluoroether elastomer; S2, passivation treatment of the devolatilized perfluoroether elastomer under swelling conditions, and removal of the passivation medium; S3, washing the passivated perfluoroether elastomer with deionized water, dehydrating it, and then vacuum drying it to obtain a devolatilized and passivated perfluoroether elastomer; S4, mixing the devolatilized and passivated perfluoroether elastomer, adding a vulcanizing agent and a filler, and compression molding; S5, radiation vulcanization of the compression-molded perfluoroether elastomer, and short-time high-temperature vulcanization to obtain a perfluoroether elastomer composition.

[0008] In one embodiment, in S1, the liquid or supercritical fluid is N2 or CO2.

[0009] In one embodiment, in S1, the liquid or supercritical fluid further contains an entrainer, and the entrainer includes at least one of methanol, ethanol, isopropanol, acetone, chloroform, hexane, and trichloroethane, and the amount of the entrainer is 0.5-10.0% of the mass of the fluid.

[0010] In one embodiment, before the devolatilization treatment in S1, the fluorodiene-modified perfluoroether elastomer is vacuum dried or freeze dried.

[0011] In one embodiment, S2 comprises: performing swelling treatment on the devolatilized perfluoroether elastomer to obtain a swollen perfluoroether elastomer; passivating the swollen perfluoroether elastomer by fluorination, the fluorinating agent comprising at least one of F2, NF3, SF4, PF5, IF5, and IF7, the v / v concentration of the fluorinating agent in the total gas is 1-10%, wherein the balance gas in the total gas is N2 or CO2.

[0012] In one embodiment, the perfluoroether elastomer is swollen with a fluid or a supercritical fluid for 2-6 hours.

[0013] In one embodiment, the temperature of fluorination passivation is 30-200° C., and the cumulative amount of passivation medium introduced per unit mass of perfluoroether elastomer polymer is 1-10 g / kg polymer.

[0014] In one embodiment, in S5, the compression molded perfluoroether elastomer is vulcanized using electron beam radiation, and the radiation dose range is 10-100 kGy.

[0015] In one embodiment, in S4, the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, with a mass fraction of 0.5-2 parts.

[0016] A fluorodiene-modified radiation-vulcanized cross-linked perfluoroether elastomer composition is prepared by the above method and is applied to semiconductor manufacturing process.

[0017] Compared with the prior art, the advantages of the present invention are: the perfluoroether elastomer is first devolatilized by liquid or supercritical fluid and then passivated under swelling conditions, thereby reducing the volatile matter in the perfluoroether elastomer; the perfluoroether elastomer after passivation treatment has excellent processability and storage stability, and is not easy to change color when exposed to high temperature and oxidative environment during subsequent processing and use; at the same time, radiation vulcanization and short-time high-temperature qualitative treatment are adopted to form a perfluoroether elastomer composition with a grid structure inside, good mechanical properties and low compression permanent deformation, and the product can be applied to high-clean semiconductor processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 The present invention is a simplified flow chart of the preparation method of the fluorodiene modified radiation vulcanized cross-linked perfluoroether elastomer composition in the embodiment of the present invention. DETAILED DESCRIPTION

[0020] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0021] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0022] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0023] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0024] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0025] Fluoroelastomer products are a versatile and multi-purpose sealing material. In high-precision chip production, trace impurities will greatly reduce the performance of chip products. Only ultra-clean, high-purity environments can meet the needs of the semiconductor industry. Fluoroelastomer products used in semiconductor processes must not only have excellent chemical resistance, thermal stability and mechanical properties, but also have low levels of extractables, low outgassing and low permeability.

[0026] However, in actual applications, fluorinated elastomers with the same chemical composition often have very different processing and application properties, and are even not suitable for practical applications. The factors that affect the processing and application properties of fluorinated elastomers and the physical properties of products mainly include chemical composition, chemical structure, polymer physical form, and the end groups of fluorinated elastomers.

[0027] Whether the end group is stable is determined by its chemical structure, which depends on the polymerization chemistry and specific polymerization conditions. Fluorine-containing elastomers, depending on the polymerization conditions such as the type of polymerization initiator and chain transfer agent used during polymerization, generate not only stable end groups such as trifluoromethyl-CF3, but also unstable end groups such as carboxylic acid-COOH, acyl fluoride-COF, hydroxymethyl-CH2OH and ester functional group-COOCH3. These unstable end groups will decompose during the subsequent high-temperature processing, and the released gas will produce bubbles, which will have an adverse effect on the processing and physical properties of the product. The prepared sealing products are used in semiconductor processes. The unstable end groups will slowly decompose, precipitate fluoride ions and other pollutants, pollute the semiconductor process, and affect the quality of semiconductor components. Fluoroether elastomers should also remove components such as initiators, chain transfer agents, emulsifiers, etc. added during the polymerization process. If perfluoroether elastomers contain a small amount of residues of these components, they are very likely to undergo oxidation and yellowing during subsequent processing and use.

[0028] Different from the treatment of thermoplastic resins such as PFA, fluoroelastomers such as perfluoroether elastomers become viscous flow when dried at a lower temperature (such as 120°C), the particles adhere to each other, the porosity decreases, the pressure difference and mass transfer resistance increase, so that the initiator, chain transfer agent, surfactant and small molecule polymer wrapped in it cannot be completely removed, that is, it cannot be effectively devolatilized, and subsequent effective end group passivation treatment cannot be carried out. This is reflected in the fact that perfluoroether elastomers produced at home and abroad at this stage are all yellow or amber after high temperature treatment.

[0029] like Figure 1 As shown, the present invention provides a method for preparing a fluorodiolefin-modified radiation-vulcanized cross-linked perfluoroether elastomer composition, comprising the following steps: S1. Devolatilization of a fluorodiene-modified perfluoroether elastomer is carried out using a liquid or a supercritical fluid; the fluorodiene-modified perfluoroether elastomer is obtained by emulsion polymerization of 43-68 parts by mass of tetrafluoroethylene, 30-55 parts by mass of perfluoroalkyl vinyl ether, 0.05-0.85 parts by mass of an iodine-containing chain transfer agent, 0.3-0.5 parts by mass of a peroxide initiator and 1-2 parts by mass of a non-conjugated fluorodiene as a vulcanization point monomer; the hyperbranched perfluoroether elastomer emulsion is coprecipitated and condensed with a PFA emulsion, and then washed to obtain a fluorodiene-modified perfluoroether elastomer.

[0030] The perfluoroether elastomer emulsion prepared by aqueous emulsion polymerization is subjected to condensation, washing and centrifugal dehydration treatment to disperse the condensation into particles while preventing them from agglomerating. The size of the resulting polymer particles is about 0.01mm-1mm, which is conducive to removing the free water and part of the bound water contained in the fluoroelastomer and keeping most of the particles from sticking to each other. In one embodiment, the fluorodiolefin-modified perfluoroether elastomer can be vacuum dried or freeze-dried before the S1 devolatilization treatment; and then the fluoroelastomer is devolatilized using liquid N2, liquid CO2, supercritical CO2 or supercritical N2; the devolatilization temperature is 25-80°C and the pressure is 7-12 MPa.

[0031] Hyperbranched perfluoroether elastomer emulsion refers to a perfluoroether elastomer in the emulsion having a large number of end groups, and the end groups are easily chemically modified. The properties of the end groups largely determine the physical and chemical properties of the hyperbranched perfluoroether elastomer.

[0032] The temperature of the emulsion polymerization is 50-90°C.

[0033] The perfluoroalkyl vinyl ether includes perfluoromethyl vinyl ether, perfluoroethyl vinyl ether, and perfluoropropyl vinyl ether, and the proportion of the perfluoroalkyl vinyl ether is 30-55 parts.

[0034] The general mechanism of fluorinated monomer and free radical polymerization is

[0035] Hyperbranched perfluoroether elastomer emulsion polymerization is achieved by controlling the branching of the polymer chain. A very small amount of highly active fluorodiolefins can also be used in the reaction medium to react with the polymer chain to form multifunctional molecules. By strictly controlling the reaction, the reaction proceeds in the desired direction. Since the fluorodiolefins are active, once added, they can quickly and completely connect with the growing chain. Therefore, the number of crosslinks in the polymer depends on the number of fluorodiolefins that are introduced into the reaction. Preferably, the degree of branching reaction is controlled by adding in stages.

[0036] Peroxide initiators are compounds containing peroxy groups (-OO-). When heated, the -OO- bond breaks and splits into two corresponding free radicals, thereby initiating monomer polymerization. Peroxide initiators are divided into two categories: inorganic peroxides and organic peroxides. Inorganic peroxide initiators include hydrogen peroxide, ammonium persulfate or potassium persulfate, and organic peroxide initiators include benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, etc.

[0037] Non-conjugated fluorodienes refer to fluorodienes that do not have a conjugated structure, with two double bonds separated by multiple single bonds, i.e. containing -C=C-(C) n -C=C- system fluorodienes (n≥2).

[0038] The English name of PFA is: Polyfluoroalkoxy, and the Chinese name is: tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer (also known as: perfluoroalkyl compound, soluble polytetrafluoroethylene).

[0039] The melting point of PFA emulsion is 290~312 ℃, the melt index is in the range of 0.8-30 g / 10min, and the molding temperature is between 350~410 ℃. Conventional processes such as compression molding, extrusion molding, and injection molding can be used for PFA resin processing.

[0040] PFA emulsion is a copolymer of tetrafluoroethylene and perfluoroalkyl vinyl ether monomers, and the solid content of the emulsion is 30-60%. Perfluoroalkyl vinyl ether monomers include perfluoromethyl vinyl ether, perfluoroethyl vinyl ether and perfluoropropyl vinyl ether. The ratio of tetrafluoroethylene to perfluoroalkyl vinyl ether monomers can be 90-99:10:1.

[0041] The principle of co-precipitation and coagulation of perfluoroether elastomer emulsion and PFA emulsion is as follows: Apply high shear force (mechanical stirring coagulation) to the coagulated perfluoroether elastomer emulsion and PFA emulsion or add inorganic acid such as HCl or HNO3 and stir vigorously to make the emulsion to be coagulated coprecipitate and coagulate into particles. The coagulated granulated product can also be thoroughly washed with deionized water and vacuum dried at 50-100 ℃.

[0042] Supercritical fluid extraction is a chemical separation method that utilizes the special solubility and good transfer characteristics of supercritical fluids near the critical point. It has both solubility similar to that of liquids and transfer characteristics similar to those of gases. Its solubility strongly depends on density, making it possible to mimic a variety of liquid solvents. Separation from solutes is also very convenient, and can be achieved by simply changing pressure or temperature.

[0043] S2. The devolatilized perfluoroether elastomer is passivated under swelling conditions and the passivation medium is removed.

[0044] In one embodiment, S2 includes the following steps: performing swelling treatment on the devolatilized perfluoroether elastomer to obtain a swollen perfluoroether elastomer; The swollen perfluoroether elastomer is passivated by fluorination, the fluorinating agent includes at least one of F2, NF3, SF4, PF5, IF5, and IF7, and the v / v concentration of the fluorinating agent in the total gas is 1-10%, wherein the balance gas in the total gas is N2 or CO2. The volume ratio of the fluorinating agent to the balance gas is 1-10:99-90, so the v / v concentration of the fluorinating agent in the total gas is 1-10%.

[0045] In one embodiment, the perfluoroether elastomer is swollen with a fluid or a supercritical fluid for 2-6 h at a swelling temperature of 30-70° C. and a pressure of 9-12 MPa.

[0046] Solid organic polymers are modified by chemical reactions of supercritical fluid-swelling solid polymer matrix. By utilizing the dispersion of supercritical fluid in polymer, the reactants are dissolved in the supercritical fluid and reacted under a certain pressure to generate new products in the polymer. Supercritical fluid molecules have strong permeability. A large amount of supercritical fluid molecules are dissolved in perfluoroether elastomer polymers, and the polymers swell. During the devolatilization process, the solute diffuses from the inside to the outside, and the supercritical fluid molecules diffuse from the outside to the inside. The volume of the polymer phase changes as the diffusion proceeds.

[0047] Under swelling conditions, the supercritical fluid carries the fluorinating agent into the perfluoroether elastomer and reacts with the active groups to undergo fluorination. In this process, the perfluoroether elastomer polymer particles can be fed in batches, and the supercritical fluid can be fed continuously. The fluorination reaction rate is affected by two factors: one is the limitation of the diffusion process, and the other is the limitation of the thermodynamic equilibrium conditions. Under certain conditions of the particle size and particle size distribution of the perfluoroether elastomer particles, the changes in the strength of the two influencing factors can ultimately be attributed to the flow rate of the supercritical fluid. Qualitatively speaking, when the flow rate is very large, it is diffusion controlled, and when the flow rate is very small, it is phase equilibrium controlled.

[0048] The thermal stability of the end groups is generally arranged in the following order: -CF3>-CONH2>-COOCH3>-CH2OH>-COF. Therefore, end group passivation is to convert unstable end groups into stable end groups through chemical treatment. For example, PFA resin is treated with 1-10% fluorine gas (nitrogen as the balance gas) for end group passivation (converted into a stable end group -CF3) and / or 50% NH3 amination (converted into a stable end group -CONH2), and finally a transparent PFA powdered resin with stable processing is obtained.

[0049] The fluoroelastomer obtained by devolatilizing the perfluoroether elastomer with liquid or supercritical fluid and then passivating it under swelling conditions has low volatile matter. The degree of end group passivation or end group stabilization can be controlled and adjusted by controlling the concentration of the passivation medium and the passivation time. The passivated perfluoroether elastomer has excellent processability and storage stability, and is not easy to change color when exposed to high temperature and oxidizing environment during subsequent processing and use. At the same time, radiation vulcanization and short-time high temperature qualitative treatment are used to form a grid structure with good mechanical properties and low compression permanent deformation. The products can be used in high-cleanliness semiconductor processes.

[0050] In one embodiment, alkane solvents and aromatic hydrocarbon solvents can be used to swell the perfluoroether elastomer.

[0051] The swollen perfluoroether elastomer is passivated by fluorination. In one embodiment, before removing the passivation medium, the cumulative amount of the passivation medium introduced per unit mass of polymer is 1-10 g / kg polymer.

[0052] The fluorinating agent includes at least one of F2, NF3, SF4, PF5, IF5, and IF7, and the v / v concentration of the fluorinating agent is 1-10%, wherein the balance gas is N2 or CO2. The flow rate of the fluorinating agent is dosed by a mass flow meter, and a back pressure valve is installed at the outlet. After decompression, it is absorbed by the alkali solution and then discharged. Thermocouples can be set at the inlet and outlet of the packed bed, and the temperature changes during the fluorination process are recorded by the thermocouples: there is a peak temperature at the outlet, and the temperature gradually drops after reaching the peak value. When it approaches the inlet temperature (the temperature difference is set to 1°C), the fluorination process is considered to be over. After the experiment, the concentration of the alkali solution is titrated, and the number of moles of the fluorinating agent consumed in the fluorination process can be calculated based on the consumed alkali solution. The temperature of fluorination passivation is 30-200°C.

[0053] The initial temperature of fluorination passivation can be set at 30 °C. As the passivation process proceeds, the bed temperature gradually increases, and the peak gradually moves toward the outlet. The temperature rise is related to the concentration and flow rate of the fluorinating agent. Generally, the bed temperature can be controlled to be lower than 110 °C by limiting the concentration and flow rate of the fluorinating agent to prevent micropowder agglomeration or local agglomeration.

[0054] S3. Wash the passivated perfluoroether elastomer with deionized water, dehydrate it, and then vacuum dry it to obtain a devolatilized and passivated perfluoroether elastomer.

[0055] S4. Mix the devolatilized and passivated perfluoroether elastomer into a thin layer, add a vulcanizing agent and a filler, and perform compression molding.

[0056] Thin-pass mixing is to adjust the roller gap of the mixing mill to 1.2-3.5 mm, allow the rubber components of the above weight proportions to pass through the roller gap, and allow them to fall into the receiving tray. After all the rubber has passed through the roller gap, the rubber on the tray is folded twice and then thin-passed. After a period of time, such as 40 minutes, vulcanizer and vulcanizing aid are added, and thin-pass mixing is continued until the surface of the mixed rubber is smooth and free of particles. The total time for thin-pass mixing is about 1 hour.

[0057] In one embodiment, the filler includes at least one of carbon nanotubes, carbon black, graphene, silicon dioxide and titanium dioxide; the vulcanizing agent includes at least one of bisphenol AF, di-tert-butyl peroxide isopropylbenzene (BIPB) and bis(2-pentanol) vulcanizing agent.

[0058] S5. Radiation vulcanization and short-time high-temperature vulcanization of the compression-molded perfluoroether elastomer to obtain a perfluoroether elastomer composition.

[0059] There are about 3000 kinds of radiation that can directly or indirectly ionize the air, and any one of them can be selected. The radiation vulcanization crosslinking can be electron beam vulcanization crosslinking or gamma ray radiation vulcanization crosslinking.

[0060] Electron beam radiation vulcanization technology is to activate elastomer molecules in the elastomer matrix through high-energy electron beams emitted by electron accelerators, generate elastomer macromolecular free radicals, and cross-link elastomer macromolecules to form a three-dimensional network structure. In addition to ions, electrons, and excited molecules, the primary chemical products formed by radiation also include free radicals and certain molecular products. These primary particles are highly active and can undergo multiple reactions such as cracking, rearrangement, electron transfer, elimination (such as dehydrogenation) and addition. Usually, radiation vulcanization crosslinking does not require the addition of vulcanizing agents and is carried out at room temperature and pressure. Compared with traditional chemical vulcanization processes, electron beam radiation vulcanization crosslinking processes can improve the aging resistance of fluoroelastomer compositions, accelerate the vulcanization rate, and improve the productivity of products. However, if only radiation vulcanization is used, the permanent compression set of the product is high.

[0061] Radiation vulcanization cross-linking combined with conventional high-temperature vulcanization cross-linking can significantly reduce the vulcanization time, improve the mechanical properties and plasma resistance of the product, and at the same time the permanent compression set of the product is low.

[0062] Fluorine-containing polymers obtained by free radical polymerization are very difficult to control in terms of molecular weight and molecular weight distribution due to the existence of coupling termination and disproportionation termination of free radicals. In the past, peroxide-cured fluoroelastomers were obtained by introducing "vulcanization point" monomers that are susceptible to free radical attack into macromolecules. For example, for peroxide vulcanization systems, the bond energy of CI bonds is low, and the iodine at the end of the polymer chain can be used to vulcanize the elastomer. It is worth noting that the mechanical stability of the cross-linked network is related to the number of end groups on each macromolecule. The more the number, the better the mechanical properties of the cross-linked network. When this type of "vulcanization point" monomer technology is used, the number of end groups on each macromolecule chain is less than 2, and the resulting vulcanized rubber is relatively poor in terms of mechanical properties, compression permanent deformation, or tolerance to high-temperature superheated water steam (gas), which cannot meet the demanding requirements of semiconductor processes for the performance of fluoroelastomer vulcanized rubber.

[0063] Using a small amount of highly active fluorodiolefin as a vulcanization site monomer in the reaction medium can form polymers with complex chain structures such as star and block copolymers. Because fluorodiolefin is active, once added, it can quickly and completely connect with the growing chain, making the number of end groups on each macromolecular chain far higher than 2. This provides the necessary conditions for radiation vulcanization crosslinking.

[0064] The above method first devolatilizes the perfluoroether elastomer with liquid or supercritical fluid and then passivates it under swelling conditions, thereby reducing the volatile matter in the perfluoroether elastomer. The perfluoroether elastomer after passivation has excellent processability and storage stability, and is not easy to change color when exposed to high temperature and oxidizing environment during subsequent processing and use. At the same time, radiation vulcanization and short-time high-temperature qualitative treatment are adopted to form a perfluoroether elastomer composition with a grid structure inside, good mechanical properties and low compression permanent deformation. The product can be used in high-cleanliness semiconductor processes.

[0065] In one embodiment, in S1, the liquid or supercritical fluid is N2 or CO2. For example, the critical temperature of CO2 fluid is 31.26°C and the critical pressure is 72.9 atm; the critical temperature of N2 fluid is -147°C and the critical pressure is 33.5 atm.

[0066] In one embodiment, in S1, the liquid or supercritical fluid further contains an entrainer, which includes at least one of methanol, ethanol, isopropanol, acetone, chloroform, hexane, and trichloroethane, and the amount of the entrainer is 0.5-10.0% of the mass of the fluid. The use of the entrainer can enhance the selectivity, solubility and extraction efficiency of the CO2 extraction process, and the entrainer can be miscible with the fluid solvent and have a volatility between the extracted substance and the supercritical component to improve its selectivity and solubility for the extraction component.

[0067] Since the concentration of the extracted components is low, the error caused by the amount of adhesion in the pipeline and container after decompression release is large. In this application, the mass difference of the perfluoroether elastomer before and after the extraction can be measured to estimate the mass of the extracted volatile components.

[0068] In one embodiment, in S2, the temperature of fluorination passivation is 30-200°C, and the cumulative amount of passivation medium introduced per unit mass of perfluoroether elastomer polymer is 1-10 g / kg polymer.

[0069] In one embodiment, in S5, electron beam radiation is used to vulcanize the molded perfluoroether elastomer, and the radiation dose range is 10-100 kGy. When the rubber is irradiated, the intermolecular crosslinking reaction and the degradation reaction occur simultaneously, that is, on the one hand, the relative molecular mass of the network macromolecules formed by intermolecular crosslinking continues to increase; on the other hand, the radiation causes the chemical bonds to break and the relative molecular mass to decrease. Therefore, the radiation dose is an important parameter for determining the radiation vulcanization and crosslinking process of the elastomer composition. The radiation dose ranges from 10 to 100 kGy. Radiation is calculated by dose. When doing the experiment, the sample is placed on a turntable, and the dose is calculated once, and finally the total dose is calculated according to the number of times.

[0070] In one embodiment, in S4, the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, with a mass fraction of 0.5-2 parts.

[0071] Preparation of perfluoroether elastomer modified by fluorodiene 650 g (about 6.5 mol; mass fraction 54.3%) tetrafluoroethylene (MW 100.01), 520 g (about 3.1 mol; mass fraction 43.4%) perfluoromethyl vinyl ether (MW 166.02), 7.5 g (about 0.017 mol; mass fraction 0.6%) chain transfer agent 1,4-diiodooctafluorobutane I(CF2)4I (MW 453.84), 5.0 g initiator ammonium persulfate (APS), and 15 g (about 0.059 mol; mass fraction 1.25%) non-conjugated fluorodienes CH2=CH-(CF2)4-CH=CH2 (MW 254.12) were emulsion polymerized to obtain a hyperbranched modified perfluoroether elastomer emulsion; the non-conjugated fluorodienes were added in batches by a metering pump at the beginning and end of the reaction, 1.5 g each time, for a total of 10 times.

[0072] Co-precipitation, condensation, washing and centrifugal dehydration with 300 ml of PFA emulsion with a solid content of about 32% (containing about 110 g of PFA) were performed to obtain about 1570 g of wet perfluoroether elastomer powder with a particle size of 0.01-1 mm.

[0073] Example 1 450 g of wet perfluoroether elastomer powder was dried in a rotary vacuum drying oven at 40 °C for 24 h with an absolute pressure of 0.01 MPa to obtain a dry polymer powder with a mass of about 270 g.

[0074] The vacuum dried powder is placed in a stainless steel inner cylinder. The cylinder body is made of a 2000-mesh stainless steel screen (Tyler mesh, about 6.5 microns). The inner cylinder is placed in an extraction device. The gap between the inner cylinder and the extraction device is sealed by a PTFE sealing gasket.

[0075] Supercritical CO2 was used as the extractant, and ethanol entrainer was added by a plunger pump, with a mass of about 4% of the mass of CO2. The supercritical CO2 temperature and pressure were 85 °C and 12 MPa, respectively, and the apparent flow rate of CO2 was 0.05 m / s. GC-MS (Agilent 8860-5977B) was used to detect the concentration of organic matter in the tail gas. When the concentration of organic matter was less than 0.01 mg / kg, the devolatilization process was stopped; the temperature and pressure of the extractant were maintained for 2 h to allow the swelling to approach equilibrium.

[0076] After the system was depressurized, the CO2 fluid was switched to a fluid containing a fluorinating agent at a pressure of 4 MPa, and fluorination treatment was carried out under swelling conditions. The concentration of the fluorinating agent was 5.0% (v / v) (N2 balance, Shanghai Fubang Chemical Co., Ltd.), the fluorination temperature was 40 °C, and the flow rate was 0.2 L / min. After the fluorination treatment, N2 was replaced to purge and remove the fluorine-containing gas in the gaps to obtain a devolatilized and fluorinated perfluoroether elastomer. The cumulative amount of fluorine gas per unit mass of polymer reaction was about 4.8 g / kg polymer.

[0077] The perfluoroether elastomer product is placed in pure water at 90°C for washing, centrifugal dehydration and then dried in a vacuum drying oven to obtain a devolatilized fluorinated perfluoroether elastomer.

[0078] The perfluoroether elastomer is mixed and kneaded into a thin layer, and 6 g of a vulcanizing agent (about 2% by mass) is added, and then the mixture is molded; Radiation vulcanization crosslinking, the crosslinking dosage is 60 kGy and high temperature vulcanization is 2 h.

[0079] The corresponding parameters were measured and the functional groups on the surface of fluoroelastomer were detected by micro-infrared (Shimadzu ATM9000).

[0080] Example 2 450 g of wet perfluoroether elastomer powder was dried in a rotary vacuum drying oven at 40 °C for 24 h with an absolute pressure of 0.01 MPa to obtain a dry polymer powder with a mass of about 270 g.

[0081] The vacuum dried powder is placed in a stainless steel inner cylinder. The cylinder body is made of a 2000-mesh stainless steel screen (Tyler mesh, about 6.5 microns). The inner cylinder is placed in an extraction device. The gap between the inner cylinder and the extraction device is sealed by a PTFE sealing gasket.

[0082] Supercritical CO2 was used as the extractant, and a plunger pump was used to add methanol entrainer, with a mass of about 4% of the mass of CO2. The supercritical CO2 temperature and pressure were 85 °C and 12 MPa, respectively, and the apparent flow rate of CO2 was 0.05 m / s. GC-MS (Agilent 8860-5977B) was used to detect the concentration of organic matter in the tail gas. When the organic matter concentration was less than 0.01 mg / kg, the devolatilization process was stopped; the extractant temperature and pressure were maintained for 2 h to allow the swelling to approach equilibrium.

[0083] After the system was depressurized, the CO2 fluid was switched to a fluid containing a fluorinating agent at a pressure of 4 MPa, and fluorination treatment was carried out under swelling conditions. The concentration of the fluorinating agent was 5% (v / v) NF3 (N2 balance, Shanghai Fubon Chemical Co., Ltd.), the fluorination temperature was 100 °C, and the flow rate was 0.2 L / min. After the fluorination treatment, N2 was replaced to purge and remove the fluorine-containing gas in the gaps to obtain a devolatilized and fluorinated perfluoroether elastomer. The cumulative amount of fluorine gas per unit mass of polymer reaction was about 4.8 g / kg polymer.

[0084] The perfluoroether elastomer product is placed in pure water at 90°C for washing, centrifugal dehydration and then dried in a vacuum drying oven to obtain a devolatilized fluorinated perfluoroether elastomer.

[0085] The perfluoroether elastomer is mixed and kneaded into a thin layer, 6 g of a vulcanizing agent (about 2% by mass) is added, and the mixture is molded; Radiation vulcanization crosslinking, the crosslinking dosage is 60 kGy and high temperature vulcanization is 2 h.

[0086] The corresponding parameters were measured and the functional groups on the surface of fluoroelastomer were detected by micro-infrared (Shimadzu ATM9000).

[0087] Comparative Example 1 450 g of wet perfluoroether elastomer powder was dried in a rotary vacuum drying oven at 40 °C for 24 h with an absolute pressure of 0.01 MPa to obtain a dry polymer powder with a mass of about 270 g.

[0088] The vacuum dried powder is placed in a stainless steel inner cylinder. The cylinder body is made of a 2000-mesh stainless steel screen (Tyler mesh, about 6.5 microns). The inner cylinder is placed in an extraction device. The gap between the inner cylinder and the extraction device is sealed by a PTFE sealing gasket.

[0089] Supercritical CO2 was used as the extractant, and an ethanol entrainer was added by a plunger pump, with a mass of about 4% of the mass of CO2. The supercritical CO2 temperature and pressure were 85 °C and 12 MPa, respectively, and the apparent flow rate of CO2 was 0.05 m / s. GC-MS (Agilent 8860-5977B) was used to detect the concentration of organic matter in the tail gas. The devolatilization process was stopped when the organic matter concentration was less than 0.01 mg / kg.

[0090] After the system is depressurized, the CO2 fluid is switched to a fluid containing a fluorinating agent at a pressure of 4 MPa without swelling. The fluorinating agent concentration is 5.0% (v / v) (N2 balance, Shanghai Fubon Chemical Co., Ltd.), the fluorination temperature is 40 °C, and the flow rate is 0.2L / min. After the fluorination treatment, the fluorinated gas in the gap is purged and removed by replacing N2 to obtain a devolatilized and fluorinated perfluoroether elastomer. The cumulative amount of fluorine gas per unit mass of polymer reaction is about 4.8 g / kg polymer.

[0091] The perfluoroether elastomer product is placed in pure water at 90°C for washing, centrifugal dehydration and then dried in a vacuum drying oven to obtain a devolatilized fluorinated perfluoroether elastomer.

[0092] The perfluoroether elastomer is mixed and kneaded into a thin layer, 12 g of a vulcanizing agent, di-2-5 (about 4% by mass) is added, and the mixture is molded; High temperature vulcanization for 24 h.

[0093] The corresponding parameters were measured and the functional groups on the surface of fluoroelastomer were detected by micro-infrared (Shimadzu ATM9000).

[0094] The functional groups on the surface of the fluoroelastomer were detected by microscopy-infrared (Shimadzu ATM9000) and deionized water leaching experiments. The number of end groups after fluorination was measured by FTIR (Shimadzu), and the weight loss was measured by a balance (Shimadzu, accuracy 0.1 mg).

[0095] Table 1 Performance test results of Examples 1-2 and Comparative Example 1

[0096] Table 2 Main test results of the examples and comparative examples of the present application

[0097] * Q / SMS 004-2024 Semiconductor equipment perfluorinated seal helium mass spectrometry vacuum leak test method, this enterprise standard can be obtained through the National Standard Information Public Service Platform.

[0098] **Q / SMS 001-2024 Test method for plasma etching resistance of perfluoroether rubber seals. This enterprise standard can be obtained through the National Standard Information Public Service Platform.

[0099] By comparing Table 1 and Table 2, it can be seen that due to the low operating temperature, the weight loss of low molecular weight polymers in the perfluoroether elastomer is not large despite the long devolatilization time. After fluorination treatment, the unstable end group is reduced by more than 90%; after the end group passivation treatment, the unstable end group -COF is basically eliminated, and the stable end group -CF3 is generated. The present invention can also adjust the passivation degree by adjusting the passivation time and / or the concentration of the passivation medium and / or the passivation temperature.

[0100] By comparing Examples 1-2 and Comparative Example 1 in Tables 1 and 2, it can be seen that the present application applies non-conjugated fluorodiolefin hyperbranching modification technology to perfluoroether elastomers, and further adopts an end group passivation method to solve the problem of poor end group stability of the perfluoroether elastomer composition. The perfluoroether elastomer composition is not easy to change color when exposed to high temperature and oxidative environment during subsequent processing and use. The prepared perfluoroether elastomer composition has the characteristic of low compression permanent set and can be applied to demanding semiconductor processes.

[0101] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a fluorodiene-modified radiation-vulcanized cross-linked perfluoroether elastomer composition, characterized in that: include: S1. Devolatilizing a fluorodiene-modified perfluoroether elastomer using a liquid or supercritical fluid; the fluorodiene-modified perfluoroether elastomer is obtained by emulsion polymerization using 43-68 parts by mass of tetrafluoroethylene, 30-55 parts by mass of perfluoroalkyl vinyl ether, 0.05-0.8 parts by mass of an iodine-containing chain transfer agent, 0.3-0.5 parts by mass of a peroxy initiator, and 1-2 parts by mass of a non-conjugated fluorodiene as a vulcanization point monomer; coprecipitating and condensing the hyperbranched perfluoroether elastomer emulsion with a PFA emulsion, and washing to obtain the fluorodiene-modified perfluoroether elastomer; S2, passivating the devolatilized perfluoroether elastomer under swelling conditions and removing the passivation medium; S3, washing the passivated perfluoroether elastomer with deionized water, dehydrating it and then vacuum drying it to obtain a devolatilized and passivated perfluoroether elastomer; S4, kneading the devolatilized and passivated perfluoroether elastomer into a thin layer, adding a vulcanizing agent and a filler, and performing compression molding; S5. Radiation vulcanization and short-time high-temperature vulcanization of the compression-molded perfluoroether elastomer to obtain a perfluoroether elastomer composition.

2. The preparation method according to claim 1, characterized in that: In S1, the liquid or supercritical fluid is N2 or CO2.

3. The preparation method according to claim 1, characterized in that: In S1, the liquid or supercritical fluid further contains an entrainer, and the entrainer includes at least one of methanol, ethanol, isopropanol, acetone, chloroform, hexane, and trichloroethane. The amount of the entrainer is 0.5-10.0% of the mass of the fluid.

4. The preparation method according to claim 1, characterized in that: Before the S1 devolatilization treatment, the fluorodiene-modified perfluoroether elastomer is vacuum dried or freeze-dried.

5. The preparation method according to claim 1, characterized in that: S2 contains: performing swelling treatment on the devolatilized perfluoroether elastomer to obtain a swollen perfluoroether elastomer; The swollen perfluoroether elastomer is passivated by fluorination, the fluorinating agent includes at least one of F2, NF3, SF4, PF5, IF5, and IF7, and the v / v concentration of the fluorinating agent in the total gas is 1-10%, wherein the balance gas in the total gas is N2 or CO2.

6. The preparation method according to claim 5, characterized in that: The perfluoroether elastomer is swollen with a fluid or supercritical fluid for 2-6 hours.

7. The preparation method according to claim 5, characterized in that: The temperature of fluorination passivation is 30-200°C, and the cumulative amount of passivation medium introduced per unit mass of perfluoroether elastomer polymer is 1-10 g / kg polymer.

8. The preparation method according to claim 1, characterized in that: In S5, the molded perfluoroether elastomer is vulcanized using electron beam radiation, and the radiation dose range is 10-100 kGy.

9. The preparation method according to claim 1, characterized in that: In S4, the vulcanizing agent is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and the mass fraction is 0.5-2 parts.

10. A fluorodiene modified radiation vulcanized crosslinked perfluoroether elastomer composition, characterized in that: The perfluoroether elastomer composition is prepared by the method according to any one of claims 1 to 9, and the perfluoroether elastomer composition is applied to semiconductor manufacturing process.