Preparation method and application of red organic long-afterglow elastic film
By adding benzoanthracene or pyrene into SEBS, the problem of insufficient performance of red organic long afterglow materials in the prior art is solved, and efficient preparation of red afterglow materials is achieved, which is suitable for multi-field applications.
Patent Information
- Application Number
- CN202411204985.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to prepare a red organic long afterglow elastic film with tensile and optical properties, which limits its application in the fields of bioimaging, flexible display and multi-color dynamic anti-counterfeiting.
Benezoanthracene or pyrene is incorporated into the flexible polymer SEBS, and a mixture solution is formed by stirring and applied to a drop-coated film. The denseness and elastic properties of SEBS are used to obtain a red organic long afterglow elastic film to achieve uniform luminescence and large-area coating of the material. cover.
A large-area film with good dynamic and adjustable red afterglow luminescence performance, high transparency, flexible and stretchable is prepared. It has excellent tensile performance and is suitable for flexible display, biodetection and anti-counterfeiting applications.
Smart Images

Figure CN118930920A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic long afterglow material preparation methods, in particular to a preparation method and application of a red organic long afterglow elastic film. Background Art
[0002] Organic long-persistent luminescence (OLPL) materials have the advantages of being easy to synthesize, functionally modified and processed, and being able to regulate persistent room-temperature phosphorescence (PRTP) through reasonable molecular design. They show potential application prospects in bioimaging, photodynamic therapy, information storage anti-counterfeiting, sensing, electroluminescent devices and security protection. However, due to the characteristics of organic compounds, room-temperature phosphorescence of a single component is difficult to achieve. Researchers have improved the organic afterglow time, luminescence brightness and afterglow color by constructing a rigid environment, crystallization, host-guest doping, H-aggregates and other methods. However, the afterglow materials prepared by these methods are generally fragile, difficult to coat over a large area and emit light uniformly, and are not flexible and difficult to stretch, which seriously limits the commercial application of such materials in flexible displays, wearable and portable electronic devices and anti-counterfeiting applications. Our research group has been committed to the development of flexible afterglow materials, and has prepared elastic afterglow films with stretchable properties by doping luminescent condensed ring materials into polymers. The films prepared by this method not only have good stretchable properties, but can also be coated on a large area, providing more space for commercial users of this type of material. However, currently only a few luminescent materials can interact with polymers, and the luminescence is relatively single, making it difficult to achieve multi-color applications.
[0003] In particular, red long afterglow has unique application prospects in biological imaging because it can reduce the self-absorption of biological tissues and the scattering of photons, thereby increasing the penetration depth and showing good biocompatibility. However, due to the influence of the energy gap law of non-radiative transitions and the low singlet-triplet intersystem crossing (ISC), the emission spectrum wavelength and emission time of most long afterglow materials are generally short, and it is difficult to obtain efficient red afterglow materials at room temperature. Therefore, there are even fewer red luminescent materials that can react with polymers. Therefore, the development of red afterglow elastic films is a problem that needs to be solved urgently in the fields of biological detection applications, flexible displays, and multi-color dynamic anti-counterfeiting. Summary of the invention
[0004] The invention provides a preparation method and application of a red organic long afterglow elastic film, so as to solve the problem that it is difficult to prepare a red organic long afterglow elastic film with good tensile properties and optical properties in the prior art.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The preparation method of the red organic long afterglow elastic film comprises the following steps: adding benzanthracene or pyrene, styrene-ethylene-butylene-styrene as solutes into a solvent, and stirring the solvent at a temperature of 60°C to 80°C to completely disperse and dissolve the solutes in the solvent, thereby forming a mixed solution; then, drop-coating the mixed solution onto a substrate to form a film, and after the film is naturally cooled at room temperature, the solvent is naturally evaporated at room temperature, thereby obtaining a red organic long afterglow elastic film.
[0007] Furthermore, in the solute, the mass ratio of benzanthracene or pyrene to styrene-ethylene-butylene-styrene is 1:200.
[0008] Furthermore, the solvent is toluene.
[0009] Furthermore, the total mass of the solute added per 1 ml of toluene is 201 mg to 402 mg.
[0010] The red organic long afterglow elastic film prepared by the preparation method of the above-mentioned red organic long afterglow elastic film is used as a flexible afterglow material in electronic devices.
[0011] The red organic long afterglow elastic film prepared by the preparation method of the above-mentioned red organic long afterglow elastic film is used as a marker in biological detection.
[0012] The invention discloses an application of the red organic long afterglow elastic film prepared by the method for preparing the red organic long afterglow elastic film as an anti-counterfeiting mark.
[0013] In the present invention, benzanthracene or pyrene is doped into a flexible polymer styrene ethylene butylene styrene (SEBS), which has a simple structure and is easy to obtain, and is doped into a flexible film as a luminophore to obtain red afterglow. The compactness of the flexible polymer SEBS is used to construct a rigid environment to suppress non-radiative transitions. More importantly, the polymer has the ability to separate oxygen, which greatly improves the room temperature phosphorescence of organic molecules and obtains a red afterglow time of up to 2 seconds. At the same time, the elasticity of the polymer is used to achieve large-area coating and stretchability of the material, and uniform light emission, providing a good basis for preparing a red organic long afterglow elastic film.
[0014] Therefore, compared with the prior art, the method for preparing a red organic long afterglow elastic film provided by the present invention can prepare a red organic long afterglow elastic film, and the prepared red organic long afterglow elastic film has good dynamically adjustable red afterglow luminescence performance, and can form a uniform, transparent, flexible and stretchable large-area film, and its stretching performance is the best among polymer long afterglow materials. The improvement of flexibility and dynamic adjustment of color will be very beneficial to the application of organic LPL materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the tensile stress-strain curve of BA@SEBS obtained in Example 1.
[0016] Figure 2 These are optical micrographs of the BA@SEBS obtained in Example 1 before and after illumination and an optical photograph showing afterglow.
[0017] Figure 3 This is the afterglow time decay curve of BA@SEBS obtained in Example 1.
[0018] Figure 4 This is the tensile stress-strain curve of PY@SEBS obtained in Example 2.
[0019] Figure 5 These are optical micrographs of the PY@SEBS obtained in Example 2 before and after illumination and an optical photograph showing afterglow.
[0020] Figure 6 This is the afterglow time decay curve of PY@SEBS obtained in Example 2.
[0021] Figure 7 The Example 1 digital pattern was created to illustrate the potential application of red and green persistence films in dynamic information encryption. DETAILED DESCRIPTION
[0022] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0023] Embodiment 1:
[0024] A method for preparing a red organic long afterglow elastic film BA@SEBS, the process is as follows:
[0025] Benzanthracene (BA) and flexible polymer styrene ethylenebutylene styrene (SEBS) were used as solutes and toluene was used as solvent. Due to the good solubility of SEBS and BA in toluene, they can be mixed well.
[0026] Among them, the manufacturer of benzanthracene is Beijing Inokai Technology Co., Ltd. (purity: 97%), and the structural formula of benzanthracene is:
[0027]
[0028] The structural formula of styrene-ethylene-butylene-styrene is
[0029]
[0030] In the solute, the mass ratio of benzanthracene to styrene-ethylene-butylene-styrene is 1:200, and the total mass of the solute added per 1 ml of toluene is 201 mg to 402 mg.
[0031] In this embodiment, 2 mg of benzanthracene, 400 mg of styrene-ethylene-butylene-styrene, and 1 ml of toluene are taken. 2 mg of benzanthracene and 400 mg of styrene-ethylene-butylene-styrene are added to 1 ml of toluene, and stirred at a temperature of 60°C to 80°C to make the benzanthracene and styrene-ethylene-butylene-styrene completely and evenly dispersed and dissolved in toluene, thereby forming a mixed solution.
[0032] Then, a glass substrate is used as a substrate, and the mixed solution is drop-coated on the glass substrate to form a thin film. After the thin film is naturally cooled at room temperature of 20-25°C, the thin film on the glass substrate is transferred to a mold, and the solvent is naturally evaporated in the mold at room temperature of 20-25°C. The residue obtained is the red organic long afterglow elastic film BA@SEBS. In the obtained red organic long afterglow elastic film BA@SEBS, BA is uniformly dispersed in SEBS, and the obtained red organic long afterglow elastic film BA@SEBS is stretchable and emits light uniformly.
[0033] The following describes the performance of the red organic long afterglow elastic film BA@SEBS prepared in this embodiment in combination with the images obtained in the experiment. During the experiment, the optical performance measurement instrument used was an Ocean Optics multi-band spectrometer, and the mechanical performance measurement instrument used was an electronic universal tensile testing machine MTS CMT4000.
[0034] Figure 1 The tensile stress-strain curve of the red organic long afterglow elastic film BA@SEBS obtained in Example 1 is shown in FIG. Figure 1 It can be seen that at a constant strain rate of 2 mm·s -1 Under the conditions of , the long afterglow material with RTP performance showed excellent stretchability and was able to be stretched to about 420% of its original length. The tensile properties of the blended material were very similar to those of pure SEBS (about 445% of its original length), indicating that even trace amounts of phosphors do not affect the tensile properties of SEBS.
[0035] Figure 2 This is a macroscopic LPL picture of the red organic long afterglow elastic film BA@SEBS obtained in Example 1 at room temperature. It can be seen that the obtained red organic long afterglow elastic film BA@SEBS emits light more evenly. Figure 2 It can be seen that when the film is excited by 365nm ultraviolet light, the fluorescent color emitted by the film is blue. After irradiation for 3 seconds, the excitation light source is turned off and the polymer film can emit red afterglow (such as Figure 2 a), in the first 1s( Figure 2 b represents the first second) the afterglow brightness of the compound is stronger, from the second second (such as Figure 2 c) and the afterglow gradually disappears, from the 3rd second (as shown in Figure 2 d), the afterglow gradually disappears. The above results show that the afterglow time of the red organic long afterglow elastic film BA@SEBS reaches about 2s, which has good afterglow performance and the whole film emits light uniformly.
[0036] The afterglow performance attenuation of the red organic long afterglow elastic film BA@SEBS of Example 1 was tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 3 shown. Figure 3 In the figure, -2s to 0s is the red organic long afterglow elastic film BA@SEBS of Example 1 under 365nm ultraviolet light, which shows photoluminescence characteristics; 0s to 10s is the red organic long afterglow elastic film BA@SEBS of Example 1 after the ultraviolet light is removed, which shows green long afterglow light, and the afterglow time is about 2s, which is similar to the afterglow time observed by the naked eye.
[0037] Based on the UV response characteristics of the red organic long-lasting elastic film BA@SEBS, a digital pattern was created to illustrate their potential application in dynamic information encryption. Phosphor and a specific ratio of SEBS were mixed as anti-counterfeiting ink to generate digital ( Figure 4 ). Under 1 second of ultraviolet light excitation, the number "89" shows a red afterglow. Due to its good wear resistance and water resistance, SEBS has the potential to be used in the production of handles for sports equipment, such as badminton rackets and table tennis rackets. In addition, the addition of phosphors enables SEBS materials to effectively present various patterns of different shapes, and ultraviolet light sources can easily verify the patterns displayed on SEBS, thereby realizing the preparation of anti-counterfeiting labels, such as Figure 4 shown.
[0038] The red organic long afterglow elastic film BA@SEBS prepared in this embodiment can be used as a red flexible afterglow material in flexible display electronic devices, wearable electronic devices, and portable electronic devices, can also be used as a red anti-counterfeiting mark, and can also be used as a red mark in biological detection.
[0039] Embodiment 2:
[0040] A method for preparing a red organic long afterglow elastic film PY@SEBS, the process is as follows:
[0041] Pyrene (PY) and the flexible polymer styrene ethylene butylenestyrene (SEBS) were used as solutes and toluene was used as solvent. Due to the good solubility of SEBS and PY in toluene, they can be mixed well.
[0042] Among them, the manufacturer of pyrene is Beijing Inokai Technology Co., Ltd. (purity: 97%), and the structural formula of pyrene is:
[0043]
[0044] The structural formula of styrene-ethylene-butylene-styrene is:
[0045]
[0046] In the solute, the mass ratio of pyrene to styrene-ethylene-butylene-styrene is 1:200, and the total mass of the solute added per 1 ml of toluene is 201 mg to 402 mg.
[0047] In this embodiment, 2 mg of pyrene, 400 mg of styrene-ethylene-butylene-styrene, and 1 ml of toluene are taken. 2 mg of pyrene and 400 mg of styrene-ethylene-butylene-styrene are added to 1 ml of toluene, and stirred at a temperature of 60°C to 80°C to make pyrene and styrene-ethylene-butylene-styrene completely and evenly dispersed and dissolved in toluene, thereby forming a mixed solution.
[0048] Then, a glass substrate is used as a substrate, and the mixed solution is drop-coated on the glass substrate to form a thin film. After the thin film is naturally cooled at room temperature of 20-25°C, the thin film on the glass substrate is transferred to a mold, and the solvent is naturally evaporated in the mold at room temperature of 20-25°C. The residue obtained is the red organic long afterglow elastic film PY@SEBS, in which PY is uniformly dispersed in SEBS, and the obtained red organic long afterglow elastic film PY@SEBS is stretchable and emits light uniformly.
[0049] The following describes the performance of the red organic long afterglow elastic film PY@SEBS prepared in this embodiment in combination with the images obtained in the experiment. The apparatus used in the experiment is the same as that in embodiment 1.
[0050] Figure 5The tensile stress-strain curve of the red organic long afterglow elastic film PY@SEBS obtained in Example 2 is shown in FIG. Figure 5 It can be seen that at a constant strain rate of 2 mm·s -1 Under the conditions of , the long afterglow material with RTP performance showed excellent stretchability and was able to be stretched to about 420% of its original length. The tensile properties of the blended material were very similar to those of pure SEBS (about 445% of its original length), indicating that even trace amounts of phosphors do not affect the tensile properties of SEBS.
[0051] Figure 6 This is the macroscopic LPL picture of the red organic long afterglow elastic film PY@SEBS obtained in Example 2 at room temperature. It can be seen that the obtained polymer film emits light more uniformly. Figure 6 It can be seen that when the film is excited by 365nm ultraviolet light, the fluorescent color emitted by the film is light yellow. After irradiation for 3 seconds, the excitation light source is turned off and the polymer film can emit a light yellow afterglow (such as Figure 6 a), in the first 1s( Figure 6 b represents the first second) the afterglow brightness of the compound is stronger, from the second second (such as Figure 6 c) and the afterglow gradually disappears, from the 3rd second (as shown in Figure 6 d), the afterglow is basically invisible. The above results show that the afterglow time of the red organic long afterglow elastic film PY@SEBS reaches about 1s, with good afterglow performance, and the whole film emits light evenly.
[0052] The afterglow performance attenuation of the red organic long afterglow elastic film PY@SEBS of Example 2 was tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 7 shown. Figure 7 In the figure, -2s to 0s is the red organic long afterglow elastic film PY@SEBS of Example 2 under 365nm ultraviolet light, which shows photoluminescence characteristics; 0s to 10s is the red organic long afterglow elastic film PY@SEBS of Example 2 after the ultraviolet light is removed, which shows green long afterglow light, and the afterglow time is about 1s, which is similar to the afterglow time observed by the naked eye.
[0053] The red organic long afterglow elastic film PY@SEBS prepared in this embodiment can be used as a red flexible afterglow material in flexible display electronic devices, wearable electronic devices, and portable electronic devices, can also be used as a red anti-counterfeiting mark, and can also be used as a red mark in biological detection.
[0054] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. The embodiments described in the present invention are merely descriptions of the preferred embodiments of the present invention, and do not limit the concept and scope of the present invention. The various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction, and such combinations should also be regarded as the contents disclosed in the present disclosure as long as they do not violate the concept of the present invention. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0055] The present invention is not limited to the specific details of the above-mentioned embodiments. Within the technical concept of the present invention and without departing from the design concept of the present invention, various modifications and improvements made to the technical solution of the present invention by technical personnel in this field should fall within the protection scope of the present invention. The technical contents for which protection is sought in the present invention have been fully recorded in the claims.
Claims
1. A method for preparing a red organic long afterglow elastic film, characterized in that: Benzanthracene or pyrene, styrene-ethylene-butylene-styrene are added as solutes into a solvent, and stirred at a temperature of 60°C to 80°C to allow the solutes to be completely dispersed and dissolved in the solvent, thereby forming a mixed solution; then, the mixed solution is drop-coated onto a substrate to form a film, and after the film is naturally cooled at room temperature, the solvent is naturally evaporated at room temperature, thereby obtaining a red organic long afterglow elastic film.
2. The method for preparing the red organic long afterglow elastic film according to claim 1, characterized in that: In the solute, the mass ratio of benzanthracene or pyrene to styrene-ethylene-butylene-styrene is 1:
200.
3. The method for preparing the red organic long afterglow elastic film according to claim 2, characterized in that: The solvent is toluene.
4. The method for preparing the red organic long afterglow elastic film according to claim 3, characterized in that: The total mass of solute added per 1 ml of toluene is 201 mg~402 mg.
5. Use of the red organic long afterglow elastic film prepared by the method for preparing the red organic long afterglow elastic film as claimed in any one of claims 1 to 4 as a flexible afterglow material in electronic devices.
6. Use of a red organic long afterglow elastic film prepared by the method for preparing a red organic long afterglow elastic film as claimed in any one of claims 1 to 4 as a marker in biological detection.
7. Use of a red organic long afterglow elastic film prepared by the method for preparing a red organic long afterglow elastic film as claimed in any one of claims 1 to 4 as an anti-counterfeiting mark.