Microcellular foaming bead prepared based on recycled polystyrene and preparation method thereof
By adding new talc powder to the polystyrene recycling material, using supercritical carbon dioxide and mold surface air-cooling and hot cutting technology to foam, and then through secondary water vapor expansion, the complexity in polystyrene recycling and utilization is solved and The performance difference problem has achieved efficient and safe preparation of high-value-added foam beads, which has improved the density and mechanical properties of the material.
Patent Information
- Application Number
- CN202411020511.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing polystyrene recycling methods are complex, dangerous, large performance differences, and consume a large amount of reagents, making it difficult to achieve high-value-added reuse that is efficient, safe and clean.
After premixing of recovered polystyrene, polystyrene and new talc powder, it is foamed through supercritical carbon dioxide injection and melt extrusion, combined with die surface air cooling and hot cutting technology, it is foamed in one piece and expanded through secondary water vapor. Adjust the expansion ratio and closed cell ratio to prepare microporous foamed beads with low density and excellent mechanical properties.
The high-value reuse of polystyrene recycling materials is realized, the process is simplified, the safety risks are reduced, the expansion ratio and closed cell ratio of foamed beads are improved, and the high value-added foamed materials are obtained.
Smart Images

Figure CN118930947A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer recycling, and in particular to a method for preparing microporous foamed beads based on recycled polystyrene. Background Art
[0002] Polystyrene is non-toxic, odorless, colorless and transparent. Its products have extremely high transparency, with a light transmittance of more than 90%, good electrical insulation, easy coloring, good processing fluidity, good rigidity and good chemical corrosion resistance. It is widely used in home appliances, packaging, electrical appliances, disposable products and other fields. At the same time, polystyrene can be prepared into foamed materials with good thermal insulation properties, which are widely used in construction, packaging, cold chain, safety protection and other fields. However, polystyrene and its foamed materials are rigid and brittle materials, which are easy to break under stress. After use, they are difficult to degrade quickly in the natural environment, consuming a lot of energy and causing serious environmental pollution. Therefore, enhancing the recycling of polystyrene is of great significance for environmental protection, energy conservation, and helping to achieve the "dual carbon" goals.
[0003] At present, the recycling of polystyrene is mainly through chemical or mechanical recycling methods to convert it into reusable styrene monomers, pellets and foamed boards. For example, Chinese invention patent CN105566670A discloses a water-phase suspension granulation method for preparing gradient flame-retardant foamable polystyrene beads based on waste polystyrene materials and its products. The invention uses suspension granulation to obtain polystyrene beads from waste polystyrene foam materials, and then obtains polystyrene insulation foam boards after pentane filling and foaming. However, this technology requires multiple operations, and the addition of pentane increases the storage risk of foamed beads.
[0004] In addition, polystyrene can be decomposed into styrene monomers by chemical degradation, but at the same time, a large amount of organic reagents will be consumed, other chemical wastes will be generated, and safety and environmental risks will be increased, which is not conducive to sustainable development. The chemical process involved in the above recycling method consumes a large amount of reagents, the processing process is complicated and has a high risk factor. Suspension granulation and pentane filling lead to a complicated preparation process and increased performance differences of the foamed beads.
[0005] CN117024889A discloses a modified expandable polystyrene recycled blended GPO-R foam material and a preparation method thereof, wherein the foam material comprises the following raw materials in mass fractions: 50-65% modified polystyrene, 20-35% recycled modified polystyrene particles, 1-4% nucleating agent, 3-6% pentane and 2-5% chain extender. The invention prepares GPO-R foam material by recycling waste polystyrene through modified expandable polystyrene and recycled polystyrene, which is beneficial to achieve low carbon emissions, reduce material costs, and ensure that the performance of the foam material meets the requirements to a certain extent. However, the consumption of recycled polystyrene is not large, and modified polystyrene is still the main raw material.
[0006] Therefore, it is challenging and valuable to seek easy-to-implement, safe, efficient, and clean methods for high value-added utilization of recycled plastics. Summary of the invention
[0007] Aiming at the problem that the recycling method of polystyrene recycled materials has poor effect, the present invention provides polystyrene microporous foamed beads with polystyrene recycled materials as the main body, and adopts extrusion foaming combined with air-cooling and hot-cutting technology, and the expansion ratio of the foamed beads can be controllably adjusted through secondary foaming to obtain foamed bead materials with high closed-cell rate, low density and excellent mechanical properties, so as to realize high-value reuse of recycled materials.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] A method for preparing microporous foamed beads based on recycled polystyrene, comprising the steps of:
[0010] Step 1, premixing recycled polystyrene, polystyrene and talcum powder, melt blending, injecting supercritical carbon dioxide therein, and obtaining a blend by melt extrusion;
[0011] Step 2, the blend is continuously blended, extruded and foamed, and then air-cooled and hot-cut on the die surface to obtain foamed beads;
[0012] Step 3, saturating the foamed beads in a high-pressure gas medium, heating them with water vapor to make them expand again, cooling, shaping and drying them to obtain the microporous foamed beads;
[0013] The microporous foamed beads include 55-95 parts of recycled polystyrene, 20-45 parts of polystyrene, 0.1-5 parts of talc powder and 1-10 parts of supercritical carbon dioxide based on 100 parts of total mass.
[0014] Preferably, the microporous expanded beads include 55-90 parts of recycled polystyrene (rPS), 20-45 parts of polystyrene (PS), 0.1-5 parts of talc, and 1-10 parts of supercritical carbon dioxide based on 100 parts by total mass.
[0015] Preferably, the amount of recycled polystyrene is 60-90 parts, and the amount of polystyrene is 10-40 parts;
[0016] Further preferably, the microporous expanded beads include 55-80 parts of recycled polystyrene, 20-45 parts of polystyrene, 0.1-5 parts of talc, and 1-10 parts of supercritical carbon dioxide based on 100 parts by total mass.
[0017] The recycled polystyrene is transparent and yellowish, and its density is 0.9-1.5g / cm 3 , the glass transition temperature is 90-110℃, and it is brittle.
[0018] The polystyrene mentioned above refers to new polystyrene material or modified new polystyrene material, with a density of 0.9-1.2 g / cm 3 , the melt index is 1-10 / 10min (200°C, 5kg), and the preferred melt index is 1-5 / 10min (200°C, 5kg).
[0019] Recycled polystyrene has problems such as low glass transition temperature, poor foaming performance, and poor secondary expansion effect. In the present invention, a small amount of new polystyrene is mixed with talcum powder to improve bubble nucleation. Through the action of supercritical carbon dioxide, melt blending extrusion foaming combined with die surface air cooling and hot cutting technology is used to obtain primary foaming beads, and the expansion ratio of the foaming beads is further controllably regulated through secondary foaming technology to obtain a foaming bead material with high closed cell rate, low density and excellent mechanical properties, thereby achieving high-value reuse of recycled materials.
[0020] Preferably, the mass fraction of talc is 0.5-5 parts, and in order to obtain a more uniform pore distribution and a higher nucleation density and a lower foam density, it is further preferably 1.0-3.0 parts.
[0021] Preferably, the mass fraction of supercritical carbon dioxide is 2-8 parts, and in order to obtain a higher expansion ratio and a more stable foaming process window, it is further preferably 3.0-6.0 parts;
[0022] Preferably, the supercritical carbon dioxide injection pressure in step 1 is 15-20 MPa to ensure smooth foaming process and avoid the phenomenon that high pressure causes pore rupture and low pressure makes it difficult for the polymer to foam.
[0023] Preferably, in step 1, the melt extrusion temperature is 160-220°C, the rotation speed is 25-40r / min, and the pressure is 7-18MPa. Ensure that the polymer is completely melted and fully mixed with the injected supercritical fluid. Preferably, the temperature is 175-200°C, the rotation speed is 30-35r / min, and the pressure is 8-12MPa.
[0024] Preferably, the blending temperature in step 2 is 140-180°C, the rotation speed is 3-30r / min, and the pressure is 7-18MPa. To avoid the phenomenon that the polymer viscosity is too low to maintain the stability of the foam cells at high temperature and it is difficult to extrude and foam at low temperature during the foaming process, preferably, the temperature is 155-170°C, the rotation speed is 30-35r / min, and the pressure is 8-12MPa.
[0025] Preferably, the pelletizing speed of the die face air-cooled hot cutting in step 2 is 50-3000 r / min, preferably 600-1600 r / min.
[0026] Preferably, the blending in step 2 is carried out in a second extrusion device connected to the first extrusion device in step 1, and the extrusion foaming is carried out in a static mixer downstream of the second extrusion device;
[0027] Preferably, the temperature of the static mixer is 140-180°C, and the die pressure is 7-20 MPa. Under this temperature and pressure, the stress state of the mixture of polymer melt and gas is guaranteed to be more stable, the discharge speed at the die is uniform, and the volume of the obtained foamed beads is ensured to be similar, preferably 155.0-170.0°C, and the pressure is 8.0-15.0 MPa.
[0028] At the pressure and temperature, the foaming process can be smoothly carried out and foam beads with high expansion ratio and closed cell rate can be obtained, ensuring that they have low density and good bead bonding after steam molding. Preferably, the expansion ratio of the foamed beads in step 2 is 15-25, and the closed cell rate is 80-95%.
[0029] Preferably, in step 3, the saturation pressure of the high-pressure gas medium is 0.1-1.5 bar, the temperature is 0-40° C., and the gas medium includes one or more of air, carbon dioxide, and nitrogen.
[0030] Preferably, in step 3, the water vapor temperature is 80-100°C and the water vapor pressure is 0.3-1.5 bar. In the step, too high a temperature will cause the foaming bead structure to collapse and shrink, while too low a temperature will be detrimental to its secondary foaming. Further preferably, in step 3, the water vapor temperature is 60-100°C,
[0031] The present invention also provides microporous foamed beads based on recycled polystyrene prepared according to the preparation method, characterized in that the expansion ratio of the microporous foamed beads is 25-60, and the closed cell ratio is 75-90%.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The simple, easy-to-operate, and highly integrated extrusion foaming technology of the present invention realizes the direct conversion and utilization of polystyrene recycled materials, and directly prepares post-consumer recycled materials into high-value-added foam beads. The prepared foam beads have a controllable expansion ratio and a high closed-cell rate, which helps them to fully expand during the steam molding process to achieve full contact between the foam beads, increase the diffusion area of the molecular chains on the surfaces of adjacent beads, improve the bonding between the foam beads, and obtain foam bead materials with high closed-cell rate, low density, and excellent mechanical properties, thereby realizing high-value reuse of recycled materials. The recycled foam bead materials can be used in the fields of packaging, cold chain transportation, building insulation, home appliances, and traffic safety protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is an optical morphology picture of the microporous foamed beads prepared in Example 1.
[0035] Figure 2 This is an electron microscope image of the internal pore structure of the microporous foam prepared in Example 1.
[0036] Figure 3 This is an electron microscope image of the surface microstructure of the microporous foamed beads prepared in Example 1.
[0037] Figure 4 This is an electron microscope image of the internal pore structure of the microporous foamed beads in Example 4.
[0038] Figure 5 This is an electron microscope image of the internal pore structure of the microporous foamed beads in Comparative Example 2. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.
[0040] The raw materials used in the following specific embodiments are all purchased from the market. The recycled polystyrene is provided by Qingdao Hailuyuan Recycling Technology Co., Ltd., which is light yellow, has a certain degree of transparency, and a glass transition temperature (T g ) is 100.6°C. General purpose polystyrene (PS: PG 383, unprocessed) was purchased from Zhenjiang Chimei Chemical Co., Ltd., with a density of 1.04 g·cm -3 , melt index is 2.7cm 3 / 10min (200℃ / 5kg). Talc powder (3000 mesh) was purchased from Changzhou Changjiang Talc Powder Factory. Carbon dioxide (CO2, purity 99.8%) was used as a physical foaming agent.
[0041] Examples 1-3 and Comparative Example 1
[0042] The added mass fractions of the above raw materials are shown in Table 1. The above raw materials of this embodiment are used to prepare post-consumer recycled polystyrene foam beads, comprising the following steps:
[0043] Step 1, mix rPS, PS and talcum powder uniformly according to the mass ratio; inject supercritical carbon dioxide into the first single screw extruder at a speed of 4.0 mL / min, the injection pressure is 18.0 MPa, the temperature of the first single screw mixing unit is set to 175°C, 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, the speed is 35 r / min, and the pressure is 10.0 MPa;
[0044] Step 2, the second single-screw extruder is connected to the second extruder, the temperature of the second single-screw mixing unit is set to 160°C, 160°C, 160°C, 160°C, 160°C, 160°C, the speed is 7r / min, and the pressure is 9.0MPa; the temperature of the static mixer is 160°C, the outlet end of the second extruder is a circular extruder die head with 4 die openings with a diameter of 1.2mm, the pressure is 9.0MPa, and the rotation speed of the rotary cutter closely fitting the die head is 1000r / min; after extrusion and pelletization, foam beads are obtained, and the foam particles are taken away from the cutter under the action of the wind force of the fan, blown out from the air cooling bin, collected, sieved, bagged and matured to obtain foam beads, whose appearance is as shown Figure 1 As shown, the internal cell structure is Figure 2 As shown, the pores inside the foamed beads are evenly distributed and have similar size distribution. Figure 3 This is the microscopic surface morphology of the foamed beads. It can be seen that the surface is dense and has no holes, which ensures that the foamed beads have a high closed-cell rate.
[0045] Table 1 Ingredients and parameters of foaming beads in Examples 1 to 3 and Comparative Example 1
[0046]
[0047] As can be seen from Table 1, the closed cell rate of the foamed beads directly prepared from pure recycled polystyrene is only 70%, and there are also problems such as low expansion ratio. After adding 10 parts of new polystyrene material, the above method can achieve the increase of the closed cell rate expansion ratio and the closed cell rate, and its secondary expansion ability is also improved.
[0048] Although the closed-cell rate of the mixed system polystyrene foam beads after one foaming can reach more than 80%, its expansion ratio is still relatively low, and it is difficult to further reduce its density to achieve further improvement in thermal insulation performance. Therefore, a secondary foaming is performed to further optimize its density and performance.
[0049] Example 4-Example 8
[0050] The difference between Examples 4 to 8 and Comparative Example 2 and Example 1 is that the expansion ratio and closed cell ratio of the foamed beads are regulated by secondary foaming technology, and the foamed beads in Example 1 are used for secondary foaming, as shown in Table 2. The specific steps are as follows:
[0051] The foaming beads in Example 1 were used for secondary foaming, and the expansion ratio of the prepared foaming beads was adjusted. The specific steps are as follows: (1) The post-consumer recycled polystyrene extruded foaming beads were saturated in an air medium, the saturation pressure was 1.0 bar, the temperature was room temperature, and the saturation time was 5.0 hours. (2) The saturated foaming beads in (1) were transported to a foaming bead pre-foaming machine through a feed introduction system, and water vapor was introduced to heat them for secondary expansion at a temperature of 80.0-105.0°C. The expansion ratio and closed cell ratio of the foaming beads after secondary expansion are shown in Table 2.
[0052] Table 2 Examples 5-8 and Comparative Example 2 are the water vapor pressure conditions during secondary foaming and the expansion ratio and closed cell ratio of the foamed beads
[0053] Serial number Secondary foaming temperature / ℃ Pressure / bar Expansion ratio Closed cell rate / % Example 4 80.0 0.50 27.0 95.0 Example 5 85.0 0.60 34.5 92.0 Example 6 90.0 0.70 42.3 87.3 Example 7 95.0 0.90 51.6 84.2 Example 8 100.0 1.00 60.0 80.2 Comparative Example 2 105.0 1.20 45.0 55.0
[0054] The internal microscopic morphology of the microporous foamed beads after secondary foaming in Example 4 is as follows: Figure 4 , it can be clearly seen that the pores are significantly enlarged. Figure 5 The electron microscope image of the internal cell structure of the microporous expanded beads in Comparative Example 2. As can be seen from Table 2, below the glass transition temperature, as the secondary expansion temperature gradually increases, the expansion ratio of the expanded beads gradually increases, and the closed cell ratio decreases. When the secondary expansion temperature is 100°C, the expansion ratio reaches 60, and the closed cell ratio is 80%. When the temperature is 105°C, since the temperature exceeds the glass transition temperature of the system, the expanded beads experience cell collapse, resulting in a low expansion ratio and a significant decrease in the closed cell ratio.
[0055] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing microporous foamed beads based on recycled polystyrene, characterized in that: Includes steps: Step 1, premixing recycled polystyrene, polystyrene and talcum powder, melt blending, injecting supercritical carbon dioxide therein, and obtaining a blend by melt extrusion; Step 2, the blend is continuously blended, extruded and foamed, and then air-cooled and hot-cut on the die surface to obtain foamed beads; Step 3, saturating the foamed beads in a high-pressure gas medium, heating them with water vapor to make them expand again, cooling, shaping and drying them to obtain the microporous foamed beads; The microporous foamed beads include 55-95 parts of recycled polystyrene, 20-45 parts of polystyrene, 0.1-5 parts of talc powder and 1-10 parts of supercritical carbon dioxide based on 100 parts of total mass.
2. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: The microporous foamed beads include 50-80 parts of recycled polystyrene, 20-50 parts of polystyrene, 0.1-5 parts of talc powder and 1-10 parts of supercritical carbon dioxide based on 100 parts of total mass.
3. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: In step 1, the supercritical carbon dioxide injection pressure is 15-20 MPa.
4. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: In step 1, the melt extrusion temperature is 160-220° C., the screw speed is 25-40 r / min, and the pressure is 7-18 MPa.
5. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: In step 2, the blending temperature is 140-180° C., the screw speed is 3-30 r / min, and the pressure is 7-18 MPa.
6. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: In step 2, blending is performed in a second extrusion device connected to the first extrusion device in step 1, and extrusion foaming is performed in a static mixer downstream of the second extrusion device; The temperature of the static mixer is 140-180°C, and the die pressure is 7-20 MPa.
7. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: The expansion ratio of the foamed beads in step 2 is 15-25, and the closed cell ratio is 80-95%.
8. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: In step 3, the saturation pressure of the high-pressure gas medium is 0.1-1.5 bar, the temperature is 0-40° C., and the gas medium includes one or more of air, carbon dioxide, and nitrogen.
9. The method for preparing microporous foamed beads based on recycled polystyrene according to claim 1, characterized in that: In step 3, the water vapor temperature is 60-100° C., and the water vapor pressure is 0.3-1.5 bar.
10. Microporous expanded beads based on recycled polystyrene prepared according to the preparation method according to any one of claims 1 to 9, characterized in that: The microporous foamed beads have an initial expansion ratio of 15-25 and a closed cell ratio of 80-95%; after secondary foaming by heating with water vapor, the expansion ratio is 25-60 and the closed cell ratio is 80-95%.
Citation Information
Patent Citations
Water-phase suspension granulation method for preparing gradient flame-retardant foamable polystyrene beads on basis of waste polystyrene materials and products of water-phase suspension granulation method
CN105566670A
Method for preparing high-foaming-ratio polymer-based foam beads by secondary foaming
CN112851999A
Polyolefin foamed bead as well as preparation method and application thereof
CN116622114A
Polystyrene-based foaming material as well as preparation method and application thereof
CN117430897A
Recycled-polystyrene foam extrudate having high nail-holding capability and preparation method therefor
WO2024124753A1