Preparation method and application of mineralized hydroxyapatite / polyacrylamide composite aerogel
By combining polyacrylamide gel matrix and amorphous calcium phosphate nanoclusters, high crystallinity hydroxyapatite nanoparticles are generated in situ, solving the problems of long mineralization cycle and poor stability and improving composite aerosol The mechanical and thermal insulation properties of glue achieve efficient thermal insulation effect.
Patent Information
- Application Number
- CN202411100140.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, mineralized hydroxyapatite has low nucleation ability and insufficient reactivity, resulting in a long mineralization period, high volume density and poor stability of composite gels, and mineralized particles are prone to aggregation, resulting in incompatibility. question.
Using the binding technology of polyacrylamide (PAAm) gel matrix and amorphous calcium phosphate (CaP) nanoclusters, the high crystallinity hydroxyapatite (HAP) nanoparticles are generated in situ through alternate impregnation and maturation reactions, which improves the Mechanical and thermal insulation properties of composite aerogels.
It significantly shortens the mineralization cycle, improves the mechanical strength and thermal stability of composite aerogels, enhances structural stability, reduces production costs, expands the application potential in the field of thermal insulation, and realizes the excellence of composite aerogels. Thermal insulation effect.
Smart Images

Figure CN118930953A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite aerogel preparation, and specifically relates to a mineralized hydroxyapatite / polyacrylamide composite aerogel and a preparation method and application thereof. Background Art
[0002] Ionic mineralized polymer gels are a promising method for preparing high-performance composite materials. The mechanical properties of the gel can be improved by introducing ionic compounds into polymer hydrogel materials for in situ assembly, followed by further coordinated growth and conversion into solid minerals anchored on the scaffold. Among them, hydroxyapatite (HAP) is a promising biomineral. As a calcium phosphate salt, it is the main inorganic component of bones and teeth and has sufficient hardness and strength to support the matrix. In addition, HAP can be synthesized under mild aqueous conditions, and its constituent ions are easily exchanged with other substances to form lattice defects. Therefore, HAP can be tightly combined with the organic matrix and induce apatite to grow into the permeable gel matrix.
[0003] Generally speaking, the formation of mineralized HAP mainly depends on the interaction between inorganic precursor ions and organic polymer molecules. Early studies have found that natural polymers such as gelatin, bacterial cellulose and silk protein can be used as mineralization templates to induce the growth of hydroxyapatite, and have been successfully applied in the fields of tissue engineering scaffolds and bone regeneration. However, the gel properties of most natural polymers are easily affected by their own physical properties and environmental media, resulting in a high volume density and poor stability of the aerogel obtained after freeze-drying of the composite gel. In order to solve this problem, polyacrylamide (PAAm) is used as an organic polymer matrix, which is a synthetic gel matrix with strong stability. PAAm is a linear polymer polymer, which is polymerized from acrylamide monomers. It contains a large number of active functional groups on the surface and is easy to form hydrogen bonds and chemical modifications. Various three-dimensional network structures such as branched or mesh structures can be obtained by graft copolymerization or cross-linking. However, PAAm's nucleation ability for minerals is not as good as that of natural polymers and its reaction activity is low, requiring a longer mineralization cycle. Therefore, it is particularly important to improve the promotion of the mineralization deposition of apatite by improving the organic matrix. In addition, the aggregation problem of mineralized particles on the surface of polymer matrix and the incompatibility caused by the huge difference in interfacial composition with organic matter remain a challenge. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a preparation method and application of mineralized hydroxyapatite / polyacrylamide composite aerogel, focusing on improving the mechanical properties and functional characteristics of composite aerogel materials, and realizing the preparation of high-performance hydroxyapatite (HAP) / organic composite aerogel by innovatively combining the mineralization technology of polyacrylamide (PAAm) gel matrix and amorphous calcium phosphate (CaP) nanoclusters.
[0005] To achieve the above object, the present invention first provides a method for preparing a mineralized hydroxyapatite / polyacrylamide composite aerogel, comprising the following steps:
[0006] S1. Preparation of amorphous calcium phosphate (CaP): stirring an ethanol solution containing calcium salt and triethylamine at room temperature, then slowly adding an ethanol solution containing phosphoric acid to the above solution for copolymerization, wherein the reaction is carried out at a calcium-phosphorus molar ratio of 1.333. After the reaction is completed, centrifugation is performed and the mixture is washed with water and ethanol. The obtained amorphous calcium phosphate (CaP) nanoparticles are redistributed in deionized water by ultrasonication to form a CaP suspension for standby use.
[0007] S2, synthesis of amorphous calcium phosphate / polyacrylamide gel PAAm / CaP: acrylamide monomer, crosslinking agent, initiator and catalyst are sequentially added to the CaP suspension prepared in S1, mixed and magnetically stirred, and transferred to a sealed polyethylene mold for polymerization reaction to form PAAm / CaP hydrogel;
[0008] S3. Synthesis of mineralized hydroxyapatite / polyacrylamide composite aerogel HAP / PAAm: The PAAm / CaP hydrogel prepared in S2 was immersed in a Tris-HCl buffer solution with a pH of 9 for a replacement reaction, and then alternately immersed in a Tris-HCl solution containing a potassium salt and a Tris-HCl solution containing a calcium salt with a pH of 9. After one immersion, it was washed with distilled water and immersed again. After the immersion, it was immersed in a CaCl2 aqueous solution with a pH of 11 for a aging reaction, and finally washed with distilled water and freeze-dried to obtain a HAP / PAAm composite aerogel.
[0009] Preferably, the stirring time in step S1 is 10-30 min, the copolymerization temperature is 2-10° C., the time is 6-12 h, the centrifugal speed is 8000-10000 rpm, the time is 10-30 min; the ultrasonic crushing power is 200-450 W, and the time is 10-30 min.
[0010] Preferably, in step S1, the calcium salt is selected from any one of calcium chloride dihydrate and calcium nitrate tetrahydrate, the concentration of the calcium salt is 0.05 mol / L, the concentration of the phosphoric acid is 0.06 mol / L, the length of the amorphous calcium phosphate CaP nanoparticles is 100-180 nm, and the surface height is 0.5-1.5 nm.
[0011] Preferably, in step S2, the mass ratio of acrylamide monomer, crosslinking agent, initiator and catalyst is 1:0.05:0.04, and the amount of the catalyst is 0.1-0.5 μL.
[0012] Preferably, in step S2, the crosslinking agent is N,N-methylenebisacrylamide, the initiator is potassium persulfate, and the catalyst is tetramethylethylenediamine.
[0013] Preferably, the concentration of the CaP suspension in step S2 is 10 mg / mL, and the mass ratio of CaP to acrylamide monomer is 1:1-4; the mixing temperature is 30° C., and the stirring time is 10-30 min; the polymerization temperature is 40-70° C., and the time is 1-5 h.
[0014] Preferably, the concentration of the Tris-HCl buffer solution in step S3 is 1-5 mol / L.
[0015] Preferably, in step S3, the potassium salt is K2HPO4·3H2O, the calcium salt is CaCl2·2H2O, the concentration ratio of potassium salt to calcium salt is 3:5, the single immersion time of the Tris-HCl solution containing potassium salt and the Tris-HCl solution containing calcium salt is 30-60 min, and the number of alternating immersions is 1-4 times; the concentration of the CaCl2 aqueous solution in step S3 is 500 mM, the temperature of the aging reaction is 30-50°C, and the time is 12-48 h.
[0016] Based on a general inventive concept, the present invention also provides a mineralized hydroxyapatite / polyacrylamide composite aerogel.
[0017] Based on a general inventive concept, the present invention also provides an application of a mineralized hydroxyapatite / polyacrylamide composite aerogel in the preparation of thermal insulation materials.
[0018] The mechanism of the composite aerogel of this scheme having excellent thermal insulation effect is as follows:
[0019] Polyacrylamide was used as the gel matrix, and amorphous calcium phosphate (CaP) nanoclusters were synthesized as mineralization nuclei to solve the problems of long mineralization cycle and uniformity of hydroxyapatite deposition. Then the CaP / PAAm gel was placed in the mineralization solution for repeated alternating immersion, and ripened in the calcium ion solution to convert the amorphous CaP into highly crystalline HAP. Finally, the HAP / PAAm composite aerogel was obtained by freeze drying. The in-situ generated hydroxyapatite nanoparticles have a significant enhancement effect on the mechanical properties of the aerogel. At the same time, the deposition of nanoparticles is conducive to improving the thermal insulation and thermal stability of the aerogel. The entire preparation process is simple and the equipment requirements are low. The in-situ method provides a new idea for the preparation of hydroxyapatite / organic composite aerogel materials with high mechanical properties.
[0020] During the preparation process, the CaP / PAAm gel was repeatedly immersed in the mineralizing solution, which caused the CaP nanoclusters to be evenly distributed in the PAAm network and gradually converted into highly crystalline HAP. Subsequently, after freeze-drying, a dense and stable HAP / PAAm composite aerogel was obtained. In this aerogel, the in-situ generated HAP nanoparticles not only significantly enhanced the mechanical strength of the aerogel, but also optimized the thermal insulation and thermal stability of the aerogel through its unique nanostructure.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) This scheme uses PAAm as a stable gel skeleton, taking advantage of its rich active functional groups and good chemical cross-linking properties to overcome the limitation that the performance of traditional natural polymer gels is easily affected by physical properties and environmental media. By synthesizing CaP nanoclusters as the initial mineralization nuclei, the mineralization cycle of HAP is significantly shortened, and the problem of uneven deposition of HAP on the surface of the polymer matrix is effectively solved.
[0023] (2) This scheme achieves the physical structure strengthening effect of composite aerogel by in situ mineralization of hydroxyapatite (HAP) nanoparticles into the polyacrylamide (PAAm) gel matrix. PAAm, as a stable gel skeleton, overcomes the limitation that the performance of traditional natural polymer gels is easily affected by physical properties and environmental media by utilizing its abundant active functional groups and good chemical cross-linking properties. Through the chemical action of polymerization, the hydroxyapatite nanoparticles are stably anchored in the organic matrix skeleton, thereby improving the structural stability of the composite aerogel.
[0024] (3) Amorphous calcium phosphate (CaP) nanoclusters are introduced as mineralized nuclei into the polyacrylamide (PAAm) gel matrix to accelerate the formation process of mineralized HAP and significantly shorten the mineralization cycle. The mineralization process of HAP in traditional methods often takes a long time, but the stable dispersion of the HAP precursor (CaP nanoclusters) in the PAAm gel of the present invention can avoid the problem of local uneven concentration that may occur in traditional methods, significantly shorten the subsequent mineralization cycle, and effectively solve the problem of uneven deposition of HAP on the surface of the polymer matrix, thereby reducing production costs, improving synthesis efficiency, and expanding the application potential of composite aerogels in the field of thermal insulation, and has good practical value.
[0025] (4) The present invention ensures the uniform distribution of HAP nanoparticles in the PAAm gel matrix through alternating impregnation and aging processes, which not only helps to improve the overall performance of the material, but also avoids the performance degradation problem caused by the aggregation of mineralized particles. The uniform distribution of HAP nanoparticles enhances the structural stability and thermal stability of the composite aerogel, providing a strong guarantee for the long-term application of composite materials.
[0026] (5) The mechanical strength and compression modulus of the HAP / PAAm composite aerogel prepared by this scheme are 4.29MPa and 7.31MPa, respectively, which are 3.1 times and 16.6 times that of pure PAAm aerogel. The residual weight content gradually increases with the increase of the inorganic phase, and the maximum residual weight is 56.5% under thermal decomposition at 800℃. In addition, the minimum thermal conductivity of the composite aerogel is 43.1mW / m·K. In addition, the thermal distribution surface of the aerogel is relatively stable, and the temperature shows a gradient decrease from bottom to top, which indicates that the internal porous structure of the composite aerogel can inhibit the conduction of heat and play a good thermal insulation role.
[0027] (6) The core of this scheme is to propose a simple, efficient, and low-equipment-demand in-situ mineralization method, which opens up a new path for the preparation of HAP / organic composite aerogel materials with excellent mechanical properties and functional characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 : Atomic force micrographs of calcium phosphate CaP in Experimental Example 1, a is a 2D atomic force micrograph, b is a 3D atomic force micrograph, and c is the surface height of the corresponding single CaP;
[0030] Figure 2 is the X-ray diffraction pattern of calcium phosphate CaP in Experimental Example 1;
[0031] Figure 3 This is the SEM image of the composite aerogel HAP / PAAm in Experimental Example 2;
[0032] Figure 4 This is the electron scanning electron microscopy image of aerogel PAAm in Experimental Example 2;
[0033] Figure 5 This is the X-ray energy spectrum elemental image analysis diagram of the composite aerogel HAP / PAAm in Experimental Example 2;
[0034] Figure 6 is the X-ray diffraction pattern of the aerogel in Experimental Example 2;
[0035] Figure 7 is a stress-strain curve of the aerogel in Experimental Example 2;
[0036] Figure 8is a thermogravimetric analysis curve of the aerogel in Experimental Example 2; a is a mass loss curve of the aerogel materials in Example 1 and Comparative Examples 1-2, and b is a weight change rate curve of the aerogel materials in Example 1 and Comparative Examples 1-2;
[0037] Fig. 9 It is the density and thermal conductivity combination diagram of aerogel in Experimental Example 3;
[0038] Fig.10 This is the infrared thermal imaging image of the aerogel in the steady state in Experimental Example 3. DETAILED DESCRIPTION
[0039] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0040] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and substance of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.
[0041] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art; unless otherwise specified, the reagents used in the examples are commercially available.
[0042] Example 1
[0043] Synthesis of HAP / PAAm composite aerogel
[0044] S1. Preparation of amorphous calcium phosphate CaP
[0045] 0.05 mol / L, 1.6 L ethanol solution of calcium chloride dihydrate and 0.2 L triethylamine were stirred at room temperature for 30 min to form a homogeneous solution. Then, 0.06 mol / L ethanol solution of phosphoric acid with a Ca / P molar ratio of 1.333 was slowly added to the above solution, and copolymerization occurred at a temperature of 4°C for 8 hours. After the reaction was completed, the amorphous calcium phosphate CaP was obtained by centrifugation at 8000 rpm for 30 minutes and rinsed with clean water and ethanol several times, and then further ultrasonically crushed in deionized water with a power of 300 W for 30 minutes. The CaP suspension was redistributed for standby use;
[0046] S2. Synthesis of amorphous calcium phosphate / polyacrylamide gel PAAm / CaP:
[0047] 2 g acrylamide monomer, 0.1 g crosslinker N,N-methylenebisacrylamide, 0.08 g initiator potassium persulfate and 0.1 μL catalyst tetramethylethylenediamine (TEMED) were added to 50 mL of 10 mg / mL CaP suspension in sequence, and mixed and dissolved under magnetic stirring at 30 °C for 30 min. Then the mixture was transferred to a sealed polyethylene mold and polymerized at 50 °C for 2 h to form PAAm / CaP hydrogel;
[0048] S3. Synthesis of mineralized hydroxyapatite / polyacrylamide composite aerogel HAP / PAAm
[0049] The PAAm / CaP hydrogel prepared by S2 was immersed in a 5mol / L tris(hydroxymethyl)aminomethane-hydrochloric acid (Tris-HCl) buffer solution (pH=9.0) for replacement reaction to keep the gel in a medium environment suitable for apatite growth. The gel was alternately immersed in a 300mM K2HPO4·3H2O Tris-HCl solution (pH=9.0) and a 500mM CaCl2·2H2O Tris-HCl solution (pH=9.0) for in-situ mineralization. The single immersion time of the Tris-HCl solution containing potassium salt and the Tris-HCl solution containing calcium salt was 30min. After immersion, the gel was washed with distilled water for 10s to remove excess ions on the surface. After 4 alternating immersions, the composite hydrogel was immersed in a 500mM CaCl2 aqueous solution (pH=11.0) and aged at a temperature of 30°C for 48h. Finally, the HAP / PAAm composite aerogel was obtained by washing with distilled water and freeze-drying.
[0050] Example 2
[0051] Synthesis of HAP / PAAm composite aerogel
[0052] S1. Preparation of amorphous calcium phosphate CaP
[0053] 0.05 mol / L, 1.6 L ethanol solution of calcium chloride dihydrate and 0.2 L triethylamine were stirred at room temperature for 20 min to form a homogeneous solution. Then, 0.06 mol / L ethanol solution of phosphoric acid with a Ca / P molar ratio of 1.333 was slowly added to the above homogeneous solution, and copolymerization occurred at a temperature of 2°C for 12 hours. After the reaction was completed, the amorphous calcium phosphate (CaP) was obtained by centrifugation at 8000 rpm for 20 min and rinsed with clean water and ethanol several times, and then further ultrasonically crushed in deionized water with a power of 450 W for 10 min. The CaP suspension was redistributed for standby use;
[0054] S2. Synthesis of amorphous calcium phosphate / polyacrylamide gel PAAm / CaP
[0055] 1.5 g acrylamide monomer, 0.075 g crosslinker N,N-methylenebisacrylamide, 0.06 g initiator potassium persulfate and 0.2 μL catalyst tetramethylethylenediamine (TEMED) were added to 50 mL of 10 mg / mL CaP suspension in sequence, and mixed and dissolved under magnetic stirring at 30 °C for 20 min. The amount of TEMED added was 0.2 μL. Then it was transferred to a sealed polyethylene mold and polymerized at 70 °C for 1 h to form PAAm / CaP hydrogel;
[0056] S3. Synthesis of mineralized hydroxyapatite / polyacrylamide composite aerogel HAP / PAAm
[0057] The CaP / PAAm hydrogel was immersed in a 4mol / L tris(hydroxymethyl)aminomethane-hydrochloric acid (Tris-HCl) buffer solution (pH=9.0) for replacement reaction to keep the gel in a medium environment suitable for apatite growth. The gel was alternately immersed in a 300mM K2HPO4·3H2O Tris-HCl solution (pH=9.0) and a 500mM CaCl2·2H2O Tris-HCl solution (pH=9.0) for in-situ mineralization. The single immersion time of the Tris-HCl solution containing potassium salt and the Tris-HCl solution containing calcium salt was 40min. After immersion, the gel was washed with distilled water for 10s to remove excess surface ions. After two alternate immersions, the composite hydrogel was immersed in a 500mM CaCl2 aqueous solution (pH=11.0) and aged at 30℃ for 36h. Finally, the HAP / PAAm composite aerogel was obtained by washing with distilled water and freeze-drying.
[0058] Example 3
[0059] Synthesis of HAP / PAAm composite aerogel
[0060] S1. Preparation of amorphous calcium phosphate CaP
[0061] 0.05 mol / L, 1.6 L ethanol solution of calcium chloride dihydrate and 0.2 L triethylamine were stirred at room temperature for 30 min to form a homogeneous solution. Then, 0.06 mol / L ethanol solution of phosphoric acid with a Ca / P molar ratio of 1.333 was slowly added to the above homogeneous solution, and copolymerization occurred at a temperature of 5°C for 10 hours. After the reaction was completed, the amorphous calcium phosphate (CaP) was obtained by centrifugation at 9000 rpm for 20 min and rinsed with clean water and ethanol several times, and then further ultrasonically crushed in deionized water with a power of 200 W for 20 min. The CaP suspension was redistributed for standby use;
[0062] S2. Synthesis of amorphous calcium phosphate / polyacrylamide gel PAAm / CaP
[0063] 1 g acrylamide monomer, 0.05 g crosslinker N,N-methylenebisacrylamide, 0.04 g initiator potassium persulfate and 0.2 μL catalyst tetramethylethylenediamine (TEMED) were added to 50 mL of 10 mg / mL CaP suspension in sequence, and mixed and dissolved under magnetic stirring at 30 °C for 20 min. Then the mixture was transferred to a sealed polyethylene mold and polymerized at 60 °C for 2 h to form PAAm / CaP hydrogel;
[0064] S3. Synthesis of mineralized hydroxyapatite / polyacrylamide composite aerogel HAP / PAAm
[0065] The CaP / PAAm hydrogel was immersed in a 3mol / L tris(hydroxymethyl)aminomethane-hydrochloric acid (Tris-HCl) buffer solution (pH=9.0) for replacement reaction to keep the gel in a medium environment suitable for apatite growth. The gel was alternately immersed in a 300mM K2HPO4·3H2O Tris-HCl solution (pH=9.0) and a 500mM CaCl2·2H2O Tris-HCl solution (pH=9.0) for in-situ mineralization. The single immersion time of the Tris-HCl solution containing potassium salt and the Tris-HCl solution containing calcium salt was 50min. After immersion, the gel was washed with distilled water for 10s to remove excess surface ions. After three alternating immersions, the composite hydrogel was immersed in a 500mM CaCl2 aqueous solution (pH=11.0) and aged at a temperature of 40℃ for 24h. Finally, the HAP / PAAm composite aerogel was obtained by washing with distilled water and freeze-drying.
[0066] Example 4
[0067] Synthesis of HAP / PAAm composite aerogel
[0068] S1. Preparation of amorphous calcium phosphate CaP
[0069] 0.05 mol / L, 1.6 L ethanol solution of calcium nitrate tetrahydrate and 0.2 L triethylamine were stirred at room temperature for 10 min to form a homogeneous solution. Then, 0.06 mol / L ethanol solution of phosphoric acid with a Ca / P molar ratio of 1.333 was slowly added to the above homogeneous solution, and copolymerization occurred at a temperature of 10°C for 12 hours. After the reaction was completed, the amorphous calcium phosphate (CaP) was obtained by centrifugation at 10000 rpm for 20 min and rinsed with clean water and ethanol several times, and then further ultrasonically crushed in deionized water with a power of 250 W for 30 min. The CaP suspension was redistributed for standby use;
[0070] S2. Synthesis of amorphous calcium phosphate / polyacrylamide gel PAAm / CaP
[0071] 0.5 g acrylamide monomer, 0.025 g crosslinker N,N-methylenebisacrylamide, 0.02 g initiator potassium persulfate and 0.2 μL catalyst tetramethylethylenediamine (TEMED) were added to 50 mL of 10 mg / mL CaP suspension in sequence, and mixed and dissolved under magnetic stirring at 30 °C for 20 min. Then the mixture was transferred to a sealed polyethylene mold and polymerized at 40 °C for 5 h to form PAAm / CaP hydrogel;
[0072] S3. Synthesis of mineralized hydroxyapatite / polyacrylamide composite aerogel HAP / PAAm
[0073] The CaP / PAAm hydrogel was immersed in a 1mol / L tris(hydroxymethyl)aminomethane-hydrochloric acid (Tris-HCl) buffer solution (pH=9.0) for replacement reaction to keep the gel in a medium environment suitable for apatite growth. The gel was alternately immersed in a 300mM K2HPO4·3H2O Tris-HCl solution (pH=9.0) and a 500mM CaCl2·2H2O Tris-HCl solution (pH=9.0) for in-situ mineralization. The single immersion time of the Tris-HCl solution containing potassium salt and the Tris-HCl solution containing calcium salt was 60min. After immersion, the gel was washed with distilled water for 10s to remove excess surface ions. After one alternating immersion, the composite hydrogel was immersed in a 500mM CaCl2 aqueous solution (pH=11.0) and aged at a temperature of 50℃ for 12h. Finally, the HAP / PAAm composite aerogel was obtained by washing with distilled water and freeze-drying.
[0074] Comparative Example 1
[0075] Preparation of pure PAAm aerogel
[0076] In Example 1, the CaP suspension and the mineralizing liquid were not added, and the remaining steps were the same as in Example 1 to prepare pure PAAm aerogel.
[0077] Comparative Example 2
[0078] Preparation of HAP / PAAm aerogel.
[0079] In Example 1, the CaP suspension was not added, and the remaining steps were the same as in Example 1 to prepare HAP / PAAm aerogel.
[0080] Experimental Example 1
[0081] Atomic force microscopy analysis and X-ray diffraction pattern of CaP prepared in Example 1
[0082] The CaP prepared in Example 1 was subjected to atomic force microscopy analysis and X-ray diffraction analysis. The results showed that Figure 1 ac are the 2D and 3D atomic force micrographs of calcium phosphate (CaP) and the surface height of a single CaP, respectively. The results show that the size and distribution of CaP clusters are relatively uniform, consisting of many well-dispersed nanoparticles with a length of about 100 to 180 nm and a surface height of about 0.5 to 1.5 nm.
[0083] From the X-ray diffraction pattern ( Figure 2 ) It can be seen that apatite has two small peaks at around 2θ=30° and 50°, but the intensity is not high. This indicates that the crystallinity of CaP is very low and it presents an amorphous structure, which is conducive to the transformation of CaP into highly crystalline hydroxyapatite in a suitable environment.
[0084] Experimental Example 2
[0085] Investigation of the properties of HAP / PAAm aerogel
[0086] (1) Scanning electron microscopy images of the aerogels prepared in Example 1 and Comparative Examples 1-2
[0087] Figure 3 The HAP / PAAm composite aerogel of Example 1, Figure 4 The scanning electron micrographs of the PAAm aerogel of Comparative Example 1 and the HAP / PAAm composite aerogel without CaP cluster mineralization of Comparative Example 2 are shown.
[0088] The results show that the pure PAAm aerogel of Comparative Example 1 presents a chaotic layer porous structure with smooth and messy pore walls. The pore walls of the HAP / PAAm composite aerogel of Comparative Example 2 have only a few slightly raised nanoparticles. Many continuous and dense small nanoparticles gradually form on the porous skeleton surface of the hydroxyapatite mineralized PAAm composite aerogel of Example 1, and the pore size structure becomes more regular, with a pore size of about 40 μm, which indicates that the calcium phosphate has been converted into a large number of hydroxyapatite nanoparticles.
[0089] Further observation of the surface element distribution of HAP / PAAm in Example 1 showed that Figure 5 As shown, the HAP / PAAm composite aerogel is mainly composed of five elements: C, O, N, Ca, and P. The Ca and P elements are evenly distributed on the pore skeleton surface of the composite aerogel, and the Ca / P ratio is about 1.67, which indicates that hydroxyapatite is successfully generated.
[0090] (2) X-ray diffraction patterns of the aerogels prepared in Example 1 and Comparative Examples 1-2
[0091] The results are as follows Figure 6As shown, the composite aerogel of Example 1 shows obvious characteristic peaks at 26.2°, 32.3°, 39.8°, 46.9°, 49.7° and 53.5°, which are attributed to the (002), (211), (300), (310), (222), (213) and (004) crystal planes of typical hydroxyapatite crystals. This verifies that hydroxyapatite gradually transforms from CaP to HAP during the mineralization process and grows in situ on the PAAm skeleton. It can be seen that compared with the pure PAAm gel of Comparative Example 1, more HAP particle crystals are gradually formed under the induction of the mineralization solution, while Comparative Example 2 without the addition of CaP clusters shows more hydroxyapatite crystal diffraction peaks, indicating that the production of apatite nanoparticles is less under mineralization.
[0092] (3) Examining the compressive stress-strain curves of the aerogels prepared in Examples 1-4 and Comparative Examples 1-2
[0093] Figure 7 The compression stress-strain curves of the HAP / PAAm composite aerogels of Examples 1-4, the pure PAAm aerogel of Comparative Example 1, and the HAP / PAAm composite aerogel of Comparative Example 2. Each sample can be compressed to 80% of its original height without breaking or cracking. The stress-strain curves of all aerogels show three stages. These compression curves all follow the typical deformation behavior of open porous structures: from linear elastic behavior at low strains to plastic yield platform and finally hardening in a high strain range. However, the maximum strength and compression modulus of the pure PAAm aerogel of Comparative Example 1 are 1.39 MPa and 0.44 MPa, respectively.
[0094] The maximum,strength and compression modulus of the composite aerogel of Experimental Example 1 are 4.29 MPa and 7.31 MPa, respectively.
[0095] This indicates that the mineralized-grown HAP nanoparticles act as a good reinforcing phase of the polymer with high strength and modulus. Meanwhile, the strong interaction between HAP and PAAm through hydrogen bonding cross-linking shows the excellent mechanical properties of the composite aerogel.
[0096] (4) Thermogravimetric curves of the aerogels prepared in Example 1 and Comparative Examples 1-2
[0097] Figure 8The thermogravimetric curves of Example 1 and Comparative Examples 1 and 2 are shown. The results show that all thermogravimetric curves mainly have three different weight loss stages, including: the weight loss in the low temperature range is caused by the evaporation of adsorbed water, the decomposition of organic components exists in the temperature range of 20-200°C, and the combustion of residual organic matrix occurs in the range of 450-600°C. When the temperature exceeds 600°C, all TG curves tend to be stable. The weight of the PAAm aerogel of Comparative Example 1 at 800°C is only 4.1%. Therefore, the percentage of hydroxyapatite in the organic / inorganic composite material can be obtained by the residual weight of the TG curve at 800°C. The amount of hydroxyapatite mineral in the composite aerogel without CaP mineralization in Comparative Example 2 is as low as 21.1%, which indicates that the degree of mineralization is poor. The mineral content in the composite aerogel of Example 1 is the largest, at 56.5%.
[0098] In addition, from Figure 8 (b) and the weight loss rate in Table 1 below show that the maximum thermal weight loss temperature of the HAP / PAAm composite aerogel of the embodiment is higher than that of the PAAm aerogel of Comparative Example 1, indicating that the hierarchical structure based on interconnected HAP can effectively inhibit the mass loss rate of degraded PAAm by reducing the heat treatment process. Therefore, the in-situ mineralized HAP / PAAm composite aerogel has higher thermal stability.
[0099] Table 1 Thermogravimetric physical parameters of gels prepared in Examples and Comparative Examples
[0100]
[0101]
[0102] In summary, amorphous CaP acts as the nucleus of organic gel mineralization. In the mineralization liquid, CaP clusters are gradually transformed into highly crystalline HAP nanoparticles and deposited in large quantities in the PAAm aerogel skeleton, forming a uniform continuous phase HAP network, and constructing a composite aerogel with a three-dimensional porous structure of nanoscale particles self-assembled. The mechanical strength and compression modulus of the obtained HAP / PAAm composite aerogel are 4.29MPa and 7.31MPa, respectively, which are 3.1 times and 16.6 times that of pure PAAm aerogel. In addition, the thermal stability of the composite aerogel gradually increases with the increase of the inorganic phase. The HAP nanoparticles deposited on the surface can effectively inhibit the heat loss of PAAm during degradation, and the maximum residual weight is 56.5% under thermal decomposition at 800℃.
[0103] Experimental Example 3
[0104] Inspecting the thermal insulation properties of the aerogels of Examples 1-4 and Comparative Example 1
[0105] like Fig. 9The volume density and thermal conductivity of the comparative example 1 and the HAP / PAAm composite aerogel are shown in Table 1. The volume density of the pure PAAm aerogel in the comparative example 1 is 0.071 g / cm 3 The volume density of HAP / PAAm composite aerogels increased relatively, which was due to the deposition of more HAP nanoparticles on the PAAm skeleton. The volume density was distributed in the range of 0.086-0.117 g / cm 3 For thermal conductivity, the thermal conductivity of PAAm aerogel is 48.05 mW / m·K, while that of HAP / PAAm is 43.1-46.5 mW / m·K, which indicates that the introduction of hydroxyapatite nanoparticles inhibits the thermal conduction of aerogel and improves the thermal insulation performance.
[0106] Further observation of the infrared thermal imaging of the composite aerogel Fig.10 As shown in the figure, the PAAm aerogel and the HAP / PAAm composite aerogel of Example 1 were placed on a hot plate heated to 100°C, and then an infrared thermal imager was used to record the infrared thermal distribution state of the aerogel in different viewing directions at steady state. It can be clearly seen from the figure that the steady-state cold surface temperature of the HAP / PAAm aerogel is about 42°C on average, which is lower than the steady-state cold surface temperature of the pure PAAm aerogel. In addition, the thermal distribution surface of the aerogel is relatively stable, and the temperature shows a gradient decrease from bottom to top, which indicates that the internal porous structure of the composite aerogel can inhibit the conduction of heat and play a good thermal insulation performance.
[0107] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a mineralized hydroxyapatite / polyacrylamide composite aerogel, characterized in that: The following steps are involved: S1. Preparation of amorphous calcium phosphate (CaP): stirring an ethanol solution containing calcium salt and triethylamine at room temperature, then slowly adding an ethanol solution containing phosphoric acid to the above solution for copolymerization, wherein the reaction is carried out at a calcium-phosphorus molar ratio of 1.
333. After the reaction is completed, centrifugation is performed and the mixture is washed with water and ethanol. The obtained amorphous calcium phosphate (CaP) nanoparticles are redistributed in deionized water by ultrasonication to form a CaP suspension for standby use. S2, synthesis of amorphous calcium phosphate / polyacrylamide gel PAAm / CaP: acrylamide monomer, crosslinking agent, initiator and catalyst are sequentially added to the CaP suspension prepared in S1, mixed and magnetically stirred, and transferred to a sealed polyethylene mold for polymerization reaction to form PAAm / CaP hydrogel; S3. Synthesis of mineralized hydroxyapatite / polyacrylamide composite aerogel HAP / PAAm: The PAAm / CaP hydrogel prepared in S2 was immersed in a Tris-HCl buffer solution with a pH of 9 for a replacement reaction, and then alternately immersed in a Tris-HCl solution containing a potassium salt and a Tris-HCl solution containing a calcium salt with a pH of 9. After one immersion, it was washed with distilled water and immersed again. After the immersion, it was immersed in a CaCl2 aqueous solution with a pH of 11 for a aging reaction, and finally washed with distilled water and freeze-dried to obtain a HAP / PAAm composite aerogel.
2. The preparation method according to claim 1, characterized in that: The stirring time in step S1 is 10-30 min, the copolymerization temperature is 2-10° C., the time is 6-12 h, the centrifugal speed is 8000-10000 rpm, the time is 10-30 min; the ultrasonic crushing power is 200-450 W, and the time is 10-30 min.
3. The preparation method according to claim 1, characterized in that: In step S1, the calcium salt is selected from any one of calcium chloride dihydrate and calcium nitrate tetrahydrate, the concentration of the calcium salt is 0.05 mol / L, the concentration of the phosphoric acid is 0.06 mol / L, the length of the amorphous calcium phosphate CaP nanoparticles is 100-180 nm, and the surface height is 0.5-1.5 nm.
4. The preparation method according to claim 1, characterized in that: In the step S2, the mass ratio of acrylamide monomer, crosslinking agent, initiator and catalyst is 1:0.05:0.04, and the amount of the catalyst is 0.1-0.5 μL.
5. The preparation method according to claim 1, characterized in that: In step S2, the crosslinking agent is N,N-methylenebisacrylamide, the initiator is potassium persulfate, and the catalyst is tetramethylethylenediamine.
6. The preparation method according to claim 1, characterized in that: The concentration of the CaP suspension in step S2 is 10 mg / mL, and the mass ratio of CaP to acrylamide monomer is 1:1-4; the mixing temperature is 30° C., and the stirring time is 10-30 min; the polymerization temperature is 40-70° C., and the time is 1-5 h.
7. The preparation method according to claim 1, characterized in that: The concentration of the Tris-HCl buffer solution in step S3 is 1-5 mol / L.
8. The preparation method according to claim 1, characterized in that: In the step S3, the potassium salt is K2HPO4·3H2O, the calcium salt is CaCl2·2H2O, the concentration ratio of the potassium salt to the calcium salt is 3:5, the single immersion time of the Tris-HCl solution containing the potassium salt and the Tris-HCl solution containing the calcium salt is 30-60 minutes, and the number of alternating immersions is 1-4 times; the concentration of the CaCl2 aqueous solution in the step S3 is 500mM, the temperature of the aging reaction is 30-50°C, and the time is 12-48h.
9. A mineralized hydroxyapatite / polyacrylamide composite aerogel prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the mineralized hydroxyapatite / polyacrylamide composite aerogel prepared by the preparation method according to any one of claims 1 to 8 in preparing thermal insulation materials.
Citation Information
Cited By
Aerogel modified based on polyphenol modified HA nanorod, and preparation method and application thereof
CN121181282A
Flame-retardant heat-insulating cellulose composite aerogel as well as preparation method and application thereof
CN122325827A
Flame-retardant thermal-insulating cellulose composite aerogels, methods of making and applications thereof
CN122325827B