Preparation method of polyimide composite aerogel for heat insulation
By introducing aluminum oxygen clusters into polyimide aerogel for covalent crosslinking, the problems of poor mechanical properties and insufficient binding force are solved, and high-efficiency insulation materials are prepared, suitable for high-temperature environments and lightweight, Dual performance of high strength and efficient heat insulation.
Patent Information
- Application Number
- CN202411184225.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
Polyimide aerogel has poor mechanical properties in high temperature environments, and insufficient binding force of cluster particles to aerogel matrix, which limits its application with dual demands of pressure and heat insulation.
Aluminum oxygen clusters are used as crosslinking agents to form an aluminum oxygen cluster composite material by covalent crosslinking with polyimide, thereby improving its mechanical properties and thermal insulation properties. The specific steps include adding aluminum oxide clusters and acid anhydride to the diamine solution, performing a condensation reaction, and then dissolving in water, lyophilizing and stage heating to form a composite aerogel.
制备出轻质高强的气凝胶材料,具备优异的隔热和力学性能,适用于高温环境,且铝氧簇的微孔结构降低了导热系数,提升了隔热性能。
Smart Images

Figure CN118930956A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a polyimide composite aerogel for heat insulation, and belongs to the technical field of functional material preparation. Background Art
[0002] With the rapid development of science and technology, high-tech fields such as aerospace, energy, microelectronics, and chemical industry have higher and higher requirements for material performance, and there is an urgent need for high-performance thermal insulation materials for high-temperature protection and reducing energy loss. Polyimide (PI) aerogel combines the performance advantages of PI resin and aerogel materials, and has excellent mechanical properties, thermal stability, heat resistance, high porosity, high specific surface area and other characteristics. It has broad application prospects in the field of thermal insulation under high temperature environments.
[0003] As a high-temperature resistant aerogel material, polyimide aerogel not only has the advantages of polyimide such as high temperature resistance, excellent thermal stability, strong mechanical properties and good flame retardant properties, but also combines the characteristics of aerogel such as light weight, high porosity and low thermal conductivity. Since the overall porosity of polyimide aerogel is as high as 90%, and the interior is composed of air and skeleton, the current compression modulus of polyimide aerogel is generally lower than 25MPa, which is manifested in that it is easy to deform or the pore structure collapses under the action of external force, and cannot be used in places with dual requirements of pressure bearing and heat insulation, which limits the application of polyimide aerogel.
[0004] Metal clusters are an emerging class of porous materials consisting of metal-containing nodes and organic ligands connected by coordination bonds. Due to their advantages such as high porosity and diverse structures, they have attracted widespread attention in gas storage and separation, air purification, energy storage, and drug delivery. At the same time, their applications still have great potential for expansion. For example, clusters are theoretically promising thermal insulation materials due to their rich microporosity and hybrid structure. The abundant micropores can inhibit gas movement and reduce the mean free path to a few nanometers (75 nanometers for free space), while the hybrid structure can scatter phonons, thereby reducing the thermal conductivity (λ). However, the thermal insulation applications of pure clusters have rarely been developed, probably because of the brittleness and difficulty in forming and processing cluster crystals.
[0005] The cluster particles and aerogel matrix are often simply physically adhered together without strong / obvious chemical bonds.
[0006] Therefore, preparing an aerogel that meets the dual requirements of high strength and thermal insulation, improving the aggregation of cluster particles and the poor compatibility of aerogel matrix and cluster particles are technical problems that need to be solved urgently. Summary of the invention
[0007] [Technical issues]
[0008] Aerogels with high porosity have poor mechanical properties;
[0009] The cluster particles have poor bonding to the aerogel substrate.
[0010] [Technical solution]
[0011] In order to solve the above problems, the present invention adopts polyimide as the substrate and uses aluminum oxide clusters as crosslinking agents between the linear molecular chains of polyimide, wherein the terminal groups of the aluminum oxide clusters are amino groups, providing sites for crosslinking with the acid anhydride in the polyimide, so that the polyimide aluminum oxide cluster composite material becomes a bulk polymer.
[0012] The first object of the present invention is to provide a method for preparing a polyimide composite aerogel for thermal insulation, comprising the following steps:
[0013] (1) dissolving a diamine in an organic solvent and stirring to obtain a diamine solution;
[0014] (2) adding aluminum oxide clusters to the diamine solution and stirring to obtain a mixed solution;
[0015] (3) adding anhydride to the mixed solution, stirring for condensation reaction, and obtaining a polyimide precursor polyamic acid solution; adding the polyimide precursor polyamic acid solution to water, washing, and drying to obtain a polymer.
[0016] (4) The polymer obtained in (3) is dissolved in water to obtain a solution, an organic compound is added to the solution to form a complex salt, the solution is frozen, dried to form, and heated in stages for thermal imidization to obtain a composite aerogel.
[0017] In one embodiment of the present invention, the preparation method of the aluminum oxide cluster in step (2) is to seal the mixture of the metal compound and the complex, react at 100° C. for 3-4 days, cool and rinse after completion to obtain crystals, namely, aluminum oxide clusters;
[0018] Wherein, the metal compound is aluminum isopropoxide, and the complex includes an internal complex and an external complex;
[0019] The inner complex is pyrazole;
[0020] The external complex is 3,4-diaminobenzoic acid or 3-aminobenzoic acid, wherein when the external complex is 3,4-diaminobenzoic acid, the prepared external complex is AlOC-18, and when the external complex is 3-aminobenzoic acid, the prepared external complex is AlOC-16;
[0021] The molar ratio of aluminum isopropoxide, pyrazole and external complex is 1:(25-30):(0.8-1.2).
[0022] In one embodiment of the present invention, the diamine in step (1) is diaminodiphenyl ether (ODA), the organic solvent is one of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), and N,N-dimethylformamide (DMF), and the concentration of the diamine solution is 20-40 mg / mL.
[0023] In one embodiment of the present invention, the stirring in step (1) is carried out at 200-300 rpm and at -2°C to 2°C for 30-60 min.
[0024] In one embodiment of the present invention, the stirring in step (2) is carried out at 200-300 rpm and at -2°C to 2°C for 30-60 min.
[0025] In one embodiment of the present invention, the solid content of the alumina clusters in step (2) (the percentage of the mass of the alumina clusters to the total mass of all solids participating in the reaction) is 1-5%.
[0026] In one embodiment of the present invention, the acid anhydride in step (3) is one of 1,2,4,5-pyromellitic dianhydride (PMDA), 4,4-oxydiphthalic anhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 4,4-oxydiphthalic anhydride.
[0027] In one embodiment of the present invention, the concentration of the anhydride in step (3) is 40-60 mg / mL.
[0028] In one embodiment of the present invention, the acid anhydride in step (3) is added in 3-6 portions and the addition is completed within 25-35 minutes.
[0029] In one embodiment of the present invention, the stirring for condensation reaction in step (3) is carried out at 200-400 rpm and 0-2° C. for 8-12 hours.
[0030] In one embodiment of the present invention, the drying in step (3) is vacuum drying or freeze drying at 30-50° C. for 5-10 h.
[0031] In one embodiment of the present invention, the solid content of the solution obtained by dissolving the polymer in water in step (4) is 6-12%.
[0032] In one embodiment of the present invention, the organic compound in step (4) is triethylamine, and its mass fraction is 5-7%.
[0033] In one embodiment of the present invention, the freezing in step (4) is freezing at -100°C to 0°C for 24-48h or freezing at -200 to -100°C for 20-30min.
[0034] In one embodiment of the present invention, the drying and forming in step (4) is performed by freeze-drying at -60°C to -30°C for 36-72 hours.
[0035] In one embodiment of the present invention, the staged heating in step (4) is carried out at 80-120, 180-220, and 230-270° C. for 50-70 min each.
[0036] In one embodiment of the present invention, the staged heating in step (4) is performed using a tubular furnace.
[0037] The second object of the present invention is to provide a composite aerogel material prepared by the above method.
[0038] The third object of the present invention is to provide application of the above method or composite aerogel material in the fields of aerospace, energy, microelectronics or chemical industry.
[0039] A fourth object of the present invention is to provide a method for improving the thermal insulation and mechanical properties of composite aerogels, comprising the following steps:
[0040] (1) dissolving a diamine in an organic solvent and stirring to obtain a diamine solution;
[0041] (2) adding aluminum oxide clusters to the diamine solution and stirring to obtain a mixed solution;
[0042] (3) adding anhydride to the mixed solution, stirring, and performing condensation reaction to obtain a polyimide precursor polyamic acid solution, adding the polyimide precursor polyamic acid solution to water, washing, and drying to obtain a polymer.
[0043] (4) The polymer obtained in (3) is dissolved in water to obtain a solution, an organic compound is added to the solution to form a complex salt, the solution is frozen, freeze-dried to form, and heat-imidized in stages to obtain a composite aerogel.
[0044] [Beneficial Effects]
[0045] (1) In the present invention, aluminum oxide clusters and polyimide are covalently cross-linked, and then freeze-dried and thermally imidized to finally prepare a lightweight and high-strength aerogel material, which takes into account the dual requirements of high strength and high-efficiency thermal insulation and has high thermal stability. Therefore, the composite aerogel has great potential in the field of flame retardancy and thermal insulation.
[0046] (2) The composite aerogel of the present invention is a very promising thermal insulation material due to its rich microporosity and hybrid structure. The rich micropores of the alumina clusters can inhibit gas migration and reduce the mean free path to a few nanometers (free space is 75 nanometers), while the hybrid structure can scatter phonons, thereby reducing the thermal conductivity, so that the thermal insulation performance of the composite aerogel is significantly improved.
[0047] (3) Cluster particles and organic matrix are usually simply physically adhered, without stable bonding. The present invention uses an alumina cluster with amino terminal groups to provide sites for bonding to polyimide and crosslink with its precursor anhydride, thus solving the problem of poor bonding between the two. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It is a bar chart of the mechanical properties of the composite aerogels in Examples 1, 2 and Comparative Example 3. DETAILED DESCRIPTION
[0049] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0050] Test method:
[0051] 1. Mechanical properties test:
[0052] The compression performance of the polyimide composite aerogel material was tested using a German Zwick Z005 Z010 Z020 universal material testing machine according to ASTM D1621 standard. The sample size was 10 mm × 10 mm × 10 mm.
[0053] 2. Thermal insulation performance test:
[0054] The thermal insulation performance of polyimide composite aerogel materials at high temperatures was tested using a Fluke TiS60+ thermal imager. The sample size was 40 mm × 40 mm × 10 mm, and the hot surface temperature was set to 200 °C.
[0055] 3. Thermal decomposition performance test:
[0056] The thermal decomposition performance test can reflect the flame retardancy and thermal stability of the composite aerogel, and the thermal decomposition performance of the composite aerogel is represented by thermogravimetric analysis. Thermogravimetric analysis (TGA) is performed on a Netzsch STA-449F3 with a temperature range of 25-800°C and a heating rate of 10°C / min in nitrogen.
[0057] The raw materials used in the embodiment:
[0058] 1,2,4,5-Pyromellitic dianhydride (PMDA, 99%), diaminodiphenyl ether (ODA, 98%), N-methylpyrrolidone (NMP, 99%), N-methylpyrrolidone (NMP, 99%), triethylamine (98%), ethanol (99.5%), triphenylphosphine (PPh3, 99%), methanol (CH3OH), and acetonitrile were purchased from Sinopharm Chemical Reagent Co., Ltd.
[0059] Cyclen (98%) and silver hexafluorophosphate (AgPF6, 99.2%) were purchased from Shanghai Bid Pharmaceutical Technology Co., Ltd.
[0060] Aluminum isopropoxide, pyrazole, and 3,4-diaminobenzoic acid were purchased from Shanghai Aladdin Reagent Co., Ltd.
[0061] Example 1
[0062] This embodiment provides a polyimide composite aerogel for thermal insulation, which is prepared by the following method:
[0063] (1) Preparation of aluminum oxide clusters:
[0064] A mixture of isopropoxide aluminum (204 mg, 1 mmol), 3,4-diaminobenzoic acid (152.15 mg, 1 mmol) and pyrazole (2 g, 29.38 mmol) was sealed in a 20 mL vial, transferred to an oven preheated to 100 °C and heated for 3 days. After the reaction was completed, it was cooled to room temperature and rinsed with ethanol to obtain reddish-brown crystals, i.e., aluminum oxide cluster AlOC-18.
[0065] (2) Preparation of PAA:
[0066] 1.2 g (6 mmol) of ODA was dissolved in 30 mL of freshly distilled NMP and stirred at 300 rpm and 0 °C for 30 min to obtain an ODA solution with a concentration of 40 mg / mL;
[0067] 0.139 g (0.066 mmol) of AlOC-18 was dissolved in the above ODA solution, the solid content of AlOC-18 was 5% (solid content = mass of AlOC-18 / (mass of ODA + mass of AlOC-18 + mass of PMDA)), and stirred at 300 rpm and 0° C. for 30 min to obtain a mixed solution;
[0068] 1.45 g (6.6 mmol) of PMDA was evenly divided into five portions and added to the mixed solution within 30 min, stirred at a constant speed (300 rpm), and condensed in an ice water bath (0° C.) for 10 h to obtain a polyimide precursor polyamic acid solution;
[0069] The obtained solution was added into 500 mL of deionized water and washed repeatedly, dried at 45° C. for 5 h, and filtered to obtain white solid polyamic acid (PAA).
[0070] (3) Preparation of composite aerogel:
[0071] Weigh 1 g of the white solid obtained in (2) and dissolve it in 9 mL of water with a solid content (the mass of PAA accounts for the total mass of the solution) of 10%, and add 2 mL of triethylamine complex salt to promote its solubility in water. Stir at room temperature, and freeze in a -40°C refrigerator for 36 hours after complete dissolution. Then, place it in a freeze dryer and freeze-dry it at -50°C for 48 hours to form it. Finally, use a tubular furnace to heat it in stages, and keep it at 100, 200, and 250°C for 1 hour each, so that the aerogel is thermally imidized to obtain a composite aerogel.
[0072] Example 2: Changing the amount of aluminum oxide clusters
[0073] The difference from Example 1 is that the addition amount of AlOC-18 in step (2) is adjusted to 1%, 2%, 3%, and 4%;
[0074] Other steps were the same as those in Example 1 to obtain a composite aerogel material.
[0075] Example 3: Different freezing temperatures
[0076] The difference from Example 1 is that the freezing in a refrigerator at -40°C in step (3) is adjusted to freezing in a liquid nitrogen (-196°C) environment, and the rest is consistent with Example 1 to obtain a composite aerogel.
[0077] Example 4: PAA solid content
[0078] The difference from Example 1 is that the PAA weighed in step (3) is adjusted to 0.6 g and dissolved in 9.4 mL of water, with a solid content of 6%. The other conditions are the same as those in Example 1 to obtain an aerogel.
[0079] Example 5: PAA solid content
[0080] The difference from Example 1 is that the PAA weighed in step (3) is adjusted to 1.2 g and dissolved in 8.8 mL of water, with a solid content of 12%. The other conditions are the same as those in Example 1 to obtain an aerogel.
[0081] Comparative Example 1: PAA solid content
[0082] The difference from Example 1 is that the PAA weighed in step (3) is adjusted to 0.5 g and dissolved in 9.5 mL of water, with a solid content of 5%. The other conditions are the same as those in Example 1 to obtain an aerogel.
[0083] Comparative Example 2: Pure polyimide aerogel
[0084] (1) Preparation of polyimide:
[0085] 1.2 g (6 mmol) of ODA was dissolved in 30 mL of freshly distilled NMP to obtain an ODA solution with a concentration of 40 mg / mL;
[0086] 1.45 g (6.6 mmol) of PMDA was evenly divided into five portions and added to the ODA solution within 30 min, and the reaction was stirred at a constant speed (300 rpm) in a water bath (0° C.) for 5 h to obtain a polyimide precursor polyamic acid solution;
[0087] The obtained solution was added into a large amount of deionized water for repeated washing, drying and filtering to obtain white solid polyamic acid PAAs.
[0088] (2) Preparation of composite aerogel:
[0089] Weigh 1 g of the white solid obtained in (1), dissolve it in 9 mL of deionized water, and add triethylamine complex salt to promote its solubility in water. After it is completely dissolved, freeze it in a -40°C refrigerator, and then put it into a freeze dryer for freeze drying. Finally, use a tubular furnace to heat the aerogel to thermally imide it to obtain a composite aerogel.
[0090] Comparative Example 3: Too high alumina addition
[0091] The difference from Example 1 is that the addition amount of AlOC-18 in step (2) is adjusted to 6% and 8%;
[0092] Other conditions and parameters are the same as in Example 1.
[0093] Comparative Example 4: Using other metal clusters
[0094] The difference from Example 1 is that AlOC-18 is replaced by a silver cluster compound, and the preparation method of the silver cluster compound is as follows:
[0095] 0.1517 g (0.6 mmol) of silver hexafluorophosphate (AgPF6) and 0.0517 g (0.3 mmol) of cyclohexanediamine (Cyclen) were weighed and dissolved in 5 mL of methanol (CH3OH) solution, and the mixture was completely dissolved by ultrasonic treatment for 1 minute to obtain a white turbid solution. 0.0262 g (0.1 mmol) of triphenylphosphine (PPh3) was added and a white turbid solution was obtained by ultrasonic treatment. 2 mL of acetonitrile was added and a light pink clear solution was obtained by ultrasonic treatment. The solution was sealed in a glass bottle and heated at 70°C for 20 hours. The solution was naturally cooled to room temperature, filtered, and the filtrate was slowly evaporated at room temperature for about one week to precipitate a large amount of colorless block crystals, which were silver clusters.
[0096] Other conditions and parameters are the same as in Example 1.
[0097] Aluminum clusters are cheaper than silver clusters, which is of great significance for reducing material costs and large-scale production; and aluminum materials have a lower density, which makes aluminum clusters and polyimide composites advantageous in applications that require lightweight materials (such as aerospace, etc.). Aluminum is one of the most abundant elements on earth and is generally considered to have less impact on the environment and human health than silver, which makes the use of aluminum clusters more environmentally friendly.
[0098] Comparative Example 5: Different order of addition
[0099] The difference from Example 1 is that in step (2), PMDA is added first and then AlOC-18 is added, specifically:
[0100] 1.2 g (6 mmol) of ODA was dissolved in 30 mL of freshly distilled NMP to obtain an ODA solution with a concentration of 40 mg / mL;
[0101] 1.45 g (6.6 mmol) of PMDA was evenly divided into five portions and added to the ODA solution within 30 min, and the reaction was stirred at a constant speed (300 rpm) in a water bath (0° C.) for 10 h to obtain a polyimide precursor polyamic acid solution;
[0102] 0.139 g (0.066 mmol) of AlOC-18 (solid content 5%) was dissolved in the polyimide precursor polyamic acid solution to obtain a mixed solution.
[0103] Comparative Example 6: Other substances with amino groups as terminal groups
[0104] The difference from Example 1 is that AlOC-18 is replaced by 1,3,5-triaminophenoxybenzene (TAB);
[0105] Other conditions and parameters are the same as in Example 1.
[0106] Example 6
[0107] The performance of the aerogels prepared in Examples 1 and 2 and Comparative Examples 1-6 was tested, and the test results are as follows:
[0108] Table 1 Mechanical properties
[0109] example Compression strength(MPa) Example 1 1.20 Example 2 (AlOC-18 addition amount 1%) 0.41 Example 2 (AlOC-18 addition amount 2%) 0.59 Example 2 (AlOC-18 addition amount 3%) 0.77 Example 2 (AlOC-18 addition amount 4%) 1.02 Example 3 1.19 Example 4 0.66 Example 5 1.22 Comparative Example 1 0.56 Comparative Example 2 0.20 Comparative Example 3 (AlOC-18 addition amount 6%) 1.06 Comparative Example 3 (AlOC-18 addition 8%) 0.99 Comparative Example 4 1.18 Comparative Example 5 0.88 Comparative Example 6 0.62
[0110] As can be seen from Table 1, the compressive strength of the composite aerogels prepared in Example 1, Example 2 (AlOC-18 addition amount 4%), Example 3 and Example 5 can reach above 1 MPa.
[0111] Table 2 Thermal insulation performance
[0112]
[0113] It can be seen from Table 2 that the temperature rise values of Example 1, Example 3 and Example 5 after 30 minutes are less than 30°C.
[0114] Table 3 Thermal insulation performance test results of Example 2 and Comparative Example 3
[0115] 1% 2% 3% 4% 6% 8% 0min 25℃ 25℃ 25℃ 25℃ 25℃ 25℃ 10min 47℃ 45℃ 42℃ 39℃ 45℃ 44℃ 30min 68℃ 64℃ 59℃ 55℃ 60℃ 66℃
[0116] It can be seen from Table 3 that if the amount of AlOC-18 added is too low or too high, the thermal insulation performance of the prepared composite aerogel will be reduced.
[0117] Table 4 Thermogravimetric analysis (TGA)
[0118]
[0119]
[0120] It can be seen from Table 4 that the composite aerogel prepared in the embodiment has a higher initial decomposition temperature and good thermal stability.
[0121] Table 5 Density of composite aerogel
[0122] <![CDATA[Density (g / cm 3 )]]> Example 1 (PAA solution solid content 10%) 0.235 Example 4 (PAA solution solid content 6%) 0.198 Example 5 (PAA solution solid content 12%) 0.322 Comparative Example 1 (PAA solution solid content 5%) 0.184
[0123] In actual application scenarios, the composite aerogel as a thermal insulation material should not only meet the good performance of flame retardancy and thermal insulation, but also meet the requirements of composite lightness, that is, the density should not exceed 0.3g / cm 3 As shown in Table 5, when the solid content of PAA increases, the density of the composite aerogel also increases. When the solid content of PAA solution is 10%, the composite aerogel not only meets the requirements of light weight, but also has good performance.
[0124] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a polyimide composite aerogel for thermal insulation, characterized in that: The steps include: (1) dissolving a diamine in an organic solvent and stirring to obtain a diamine solution; (2) adding aluminum oxide clusters to the diamine solution and stirring to obtain a mixed solution; (3) adding anhydride to the mixed solution, stirring for condensation reaction, obtaining a polyimide precursor polyamic acid solution, adding the polyimide precursor polyamic acid solution to water, washing, and drying to obtain a polymer; (4) The polymer obtained in (3) is dissolved in water to obtain a solution, an organic compound is added to the solution to form a complex salt, the solution is frozen, dried to form, and heated in stages for thermal imidization to obtain a composite aerogel.
2. The method according to claim 1, characterized in that The concentration of the diamine solution in step (1) is 20-40 mg / mL.
3. The method according to claim 1, characterized in that The solid content of the aluminum oxide cluster in step (2) is 1-5%.
4. The method according to claim 1, characterized in that: The concentration of the anhydride in step (3) is 40-60 mg / mL.
5. The method according to claim 1, characterized in that In step (3), the acid anhydride is added in 3-6 portions and the addition is completed within 25-35 minutes.
6. The method according to claim 1, characterized in that In step (4), the solid content of the solution obtained by dissolving the polymer in water is 6-12%.
7. The method according to claim 1, characterized in that The freezing in step (4) is performed at -100°C to 0°C for 24-48 hours or at -200°C to -100°C for 20-30 minutes.
8. A composite aerogel material, characterized in that: The method is prepared by any one of claims 1 to 7.
9. Application of the composite aerogel material according to claim 8 in the fields of aerospace, energy, microelectronics or chemical industry.
10. A method for improving the thermal insulation and mechanical properties of composite aerogels, characterized in that: The steps include: Preparation of polyimide and alumina polymer: (1) dissolving a diamine in an organic solvent and stirring to obtain a diamine solution; (2) adding aluminum oxide clusters to the diamine solution and stirring to obtain a mixed solution; (3) adding anhydride to the mixed solution, stirring, and performing condensation reaction to obtain a polyimide precursor polyamic acid solution, adding the polyimide precursor polyamic acid solution to water, washing, and drying to obtain a polymer. Preparation of composite aerogel: (4) The polymer obtained in (3) is dissolved in water to obtain a solution, an organic compound is added to the solution to form a complex salt, the solution is frozen, freeze-dried to form, and heat-imidized in stages to obtain a composite aerogel.
Citation Information
Cited By
Preparation method of moisture-proof and heat-insulating polyimide composite aerogel
CN119955172A