Polyimide / fiber composite aerogel as well as preparation method and application thereof
By preparing polyimide/fiber composite aerogels, the problems of high strength and high porosity were solved, and the effective composite of fibers and polyimide was achieved, which improved the mechanical properties and thermal stability of the aerogels while reducing thermal conductivity.
Patent Information
- Application Number
- CN202411228406.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies make it difficult to prepare polyimide/fiber composite aerogels with both high strength and high porosity. Furthermore, it is difficult to form a good interface between inorganic fibers and polyimide, which leads to aerogel structure collapse and performance degradation.
Polyimide/fiber composite aerogels were prepared by dissolving fibers in an organic solvent, adding a coupling agent, mixing the solution, reacting it with diamine and dianhydride to form a precursor solution, adding a crosslinking agent, catalyst and dehydrating agent, and then performing gradient solvent replacement and supercritical CO2 drying.
It improves the mechanical properties and porosity of aerogels, reduces shrinkage, and significantly reduces thermal conductivity by forming interfacial thermal resistance through fiber filling.
Smart Images

Figure CN118930957A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic material preparation, and in particular to a polyimide / fiber composite aerogel and a preparation method and application thereof. Background Art
[0002] Polyimide (PI) is a type of macromolecular polymer with an imide group in the main chain. The main chain contains a five-membered heterocyclic ring and an aromatic ring. The molecular chain is highly rigid and has a high conjugation effect of the aromatic ring. Due to these unique structural characteristics, PI exhibits excellent performance, such as high mechanical strength, thermal stability, and low thermal conductivity. PI aerogel is a three-dimensional porous structure material composed of polymer molecular chains. It combines the outstanding properties of polyimide and aerogel. Therefore, the aerogel has the advantages of high mechanical strength and low thermal conductivity. However, it still has high shrinkage and uncontrollable pore structure, which leads to the collapse of the aerogel structure and makes it impossible to prepare high-porosity aerogel.
[0003] In the prior art, the crosslinking degree and mechanical properties of PI aerogel are improved by adding fibers. For example, the Chinese invention patent with publication number CN112830760 A involves the composite between SiO2 aerogel and fiber. A coupling agent is added between the surface of the initial SiO2 gel and the surface of each layer of fiber preform, which realizes the effective composite of SiO2 particles on the fiber surface. However, the SiO2 particles cannot be effectively composited inside the fiber, and the SiO2 particles themselves are fragile. In actual application, there is a problem of insulation failure due to the breakage and shedding of SiO2 particles. This is also the key difference between inorganic aerogel and organic aerogel. Organic aerogel is flexible, elastic, and has a certain tensile strength. Although the publication number CN 113717429 A prepares aramid fiber composite polyimide aerogel materials, and the hydrogen bond can be constructed between the two without a coupling agent, other high-temperature resistant inorganic fibers are not involved in the preparation process, such as aluminum silicate fiber, graphite fiber, ultrafine high-silica fiber, aluminum silicate ceramic fiber, carbon fiber, glass fiber, polycrystalline mullite fiber, high-purity quartz fiber, basalt fiber or polycrystalline alumina fiber, etc. In the absence of a coupling agent, it is difficult to form a good interface between the inorganic fiber and the polyimide, and thus it is impossible to obtain a polyimide / fiber composite aerogel with both high strength and high porosity. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to propose a polyimide / fiber composite aerogel and its preparation method and application, and to improve the mechanical properties of PI aerogel and reduce its shrinkage rate through a simple and efficient preparation method, so as to prepare a polyimide / fiber composite aerogel with high strength and high porosity.
[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a polyimide / fiber composite aerogel, comprising the following steps:
[0007] S1: dissolving the fiber in an organic solvent, then adding a coupling agent and stirring to obtain a fiber solution;
[0008] S2: dissolving the diamine in an organic solvent, then adding dianhydride and stirring to form a precursor solution;
[0009] S3: mixing the fiber solution in S1 with the precursor solution in S2 to form a mixed solution;
[0010] S4: adding a crosslinking agent, a catalyst and a dehydrating agent to the mixed solution in S3 in sequence to react, and obtaining a PI / fiber wet gel after drying;
[0011] S5: gradient solvent replacement of the PI / fiber wet gel in S4;
[0012] S6: The PI / fiber wet gel after gradient solvent replacement in S5 is subjected to CO2 supercritical drying to obtain a polyimide / fiber composite aerogel.
[0013] In some other embodiments, in step S1, the organic solvent is N-methylpyrrolidone or N,N-dimethylformamide;
[0014] The fiber is molybdenum fiber, aluminum silicate fiber, graphite fiber, ultrafine high silica fiber, aluminum silicate ceramic fiber, carbon fiber, glass fiber, high-purity quartz fiber, basalt fiber or polycrystalline alumina fiber, aramid fiber or polyamide fiber;
[0015] The coupling agent is a silane coupling agent;
[0016] Preferably, the silane coupling agent is KH-550, KH-792 or KH-151.
[0017] In some other embodiments, in step S1, the usage ratio of the organic solvent, fiber, and coupling agent is (1-20) mL: (0.5-2.0) g: (0.5-0.25) mL.
[0018] In some other embodiments, in step S2, the diamine is one or more of p-phenylenediamine, 2,2-diaminobenzidine or 4,4-diaminodiphenyl ether;
[0019] The dianhydride is one or both of biphenyltetracarboxylic dianhydride and pyromellitic dianhydride;
[0020] The organic solvent is N-methylpyrrolidone or N,N-dimethylformamide;
[0021] Preferably, the usage ratio of the organic solvent, diamine and dianhydride is (1-20) mL: (0.5-1.0) g: (1.0-1.5) g.
[0022] In some other embodiments, in step S4, the cross-linking agent is 1,3,5-benzenetricarboxylic acid chloride or 1,3,5-tris(4-aminophenoxy)benzene;
[0023] The catalyst is pyridine or quinoline, triethylamine or isoquinoline;
[0024] The dehydrating agent is acetic anhydride, benzoic anhydride, trifluoroacetic anhydride or succinic anhydride.
[0025] In some other embodiments, in step S4,
[0026] The usage ratio of the cross-linking agent, the catalyst and the dehydrating agent is (0.01-0.025) g: (2-5) mL: (3-10) mL.
[0027] In some other embodiments, in step S5, the specific steps of replacing the gradient solution are:
[0028] (1) Soaking in 70-90wt.% N-methylpyrrolidone ethanol solution for 12-48h;
[0029] (2) soaking in 20-50wt.% N-methylpyrrolidone ethanol solution for 12-48h;
[0030] (3) Soak in ethanol solution for 12h-48h.
[0031] In some other embodiments, in step S6, the CO2 supercritical drying condition is: the temperature is 40-60°C; preferably, the temperature is 45-55°C;
[0032] The drying pressure is 8-10Mpa; preferably, the drying pressure is 8-8.5Mpa;
[0033] The drying time is 6 to 8 hours.
[0034] In a second aspect, the present invention provides a polyimide / fiber composite aerogel prepared by the preparation method described in the first aspect, wherein the polyimide / fiber composite aerogel has a tensile strength of 0.9-1.87 MPa, a shrinkage rate of 4-9.2%, and a porosity of 83-91%.
[0035] In a third aspect, the present invention provides applications of the polyimide / fiber composite aerogel described in the second aspect in thermal insulation, oil-water separation, pressure sensing, and electromagnetic protection.
[0036] It can be seen from the above technical solution that the present invention has achieved the following beneficial effects:
[0037] (1) The present invention composites the fiber and the PI aerogel through chemical bonds. The fiber can reduce the high shrinkage of the PI aerogel and improve the porosity, mechanical properties and high-temperature thermal stability of the PI aerogel. At the same time, the fiber added as a filler can interrupt the polyimide continuous phase and form an interface thermal resistance, thereby greatly reducing the thermal conductivity of the composite material. The fiber is filled in the PI to increase the porosity of the aerogel and greatly reduce the high shrinkage of the PI.
[0038] (2) The fiber / polyimide composite aerogel prepared by the present invention has the advantages of high mechanical properties and high porosity. The tensile strength of the polyimide / fiber composite aerogel is 0.9-1.87Mpa, the shrinkage rate is 4-9.2%, and the porosity is 83-91%. At the same time, the intrinsic properties of the polyimide aerogel are not significantly affected. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 is an optical picture of the PI / fiber aerogel of Example 1 of the present invention;
[0040] Figure 2 is an optical picture of the PI aerogel of Comparative Example 1 of the present invention;
[0041] Figure 3 is the SEM image of the PI / fiber aerogel of Example 1. DETAILED DESCRIPTION
[0042] The present invention is further described in conjunction with specific examples. The following examples are only for explaining the present invention and are not intended to limit the content thereof. If the specific experimental conditions are not specified in the examples, they are usually carried out according to conventional conditions or the conditions recommended by the sales company; unless otherwise specified in the present invention, the following solvents can be purchased through commercial channels.
[0043] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0044] Example 1
[0045] (1) At 25°C, 2.0 g of aramid fiber was dissolved in 20 ml of N-methylpyrrolidone (NMP) solution, and then 0.25 mL of KH-550 was added and stirred for 1 h to obtain a fiber solution;
[0046] (2) Dissolve 0.843 g of 4,4-diaminodiphenyl ether (ODA) in 10 mL of NMP solution, then add 1.278 g of biphenyltetracarboxylic dianhydride (BPDA) and stir to dissolve to form a precursor solution; mix the fiber solution in step (1) with the precursor solution and stir for 10 min to form a mixed solution; add 5 mL of trifluoroacetic anhydride and 2.80 mL of pyridine to the mixed solution in sequence, stir for 3 min, and then quickly add 4.269 mL of NMP solution containing 0.019 g of 1,3,5-tris(4-aminophenoxy)benzene (TAB), stir for 5 min, and heat in a 50°C water bath for 30 min to obtain a PI / fiber wet gel;
[0047] (3) soaking the fiber / PI wet gel in step (2) in an ethanol solution containing 70% NMP by mass for 24 h, soaking it in an ethanol solution containing 30% NMP for 24 h, and finally aging it in the ethanol solution for 48 h (changing it every 24 h);
[0048] (4) The aged fiber / PI wet gel is subjected to CO2 supercritical drying to obtain PI / fiber aerogel.
[0049] Figure 1 This is an optical picture of the prepared PI / fiber composite aerogel. It can be clearly seen from the picture that the PI / fiber aerogel has a smooth surface and good blockiness. According to the ASTM D882-18 standard, the third-party test results show that the compressive strength of the PI / fiber composite aerogel prepared in Example 1 is 1.87MPa and the shrinkage rate is 4.1%, indicating that fiber filling significantly enhances the shrinkage resistance of the PI aerogel.
[0050] Figure 3 The SEM image of the prepared PI / fiber composite aerogel shows that the porosity of the composite aerogel filled with fibers is uniform and dense. According to the GB / T 21650.1-2008 standard, the third-party test result is 91%.
[0051] Example 2
[0052] (1) At 25°C, 1.5 g of aramid fiber was dissolved in 20 ml of NMP solution, and then 0.25 mL of KH-550 was added and stirred for 1 h to obtain a fiber solution;
[0053] (2) Dissolve 0.843 g of 4,4-diaminodiphenyl ether (ODA) in 10 mL of NMP solution, then add 1.313 g of BTDA and stir to dissolve to form a precursor solution; mix the fiber solution in step (1) with the precursor solution and stir for 10 min to form a mixed solution; quickly add 3.28 mL of acetic anhydride and 3.0 mL of triethylamine to the mixed solution in sequence, stir for 3 min, then quickly add 4.269 mL of NMP solution containing 0.019 g of 1,3,5-tris(4-aminophenoxy)benzene (TAB), stir for 5 min, then heat in a 50°C water bath for 30 min to obtain a PI / fiber wet gel;
[0054] (3) soaking the fiber / PI wet gel in step (2) in an ethanol solution containing 75% NMP by mass for 24 h, soaking it in an ethanol solution containing 25% NMP for 24 h, and finally aging it in the ethanol solution for 48 h (changing it every 24 h);
[0055] (4) The aged fiber / PI wet gel is subjected to CO2 supercritical drying to obtain PI / fiber aerogel.
[0056] The stress-strain test results show that the compressive strength of PI aerogel is 1.21 MPa, the shrinkage rate is 5.2%, and the porosity is 90.4%.
[0057] Example 3
[0058] (1) At 25°C, 0.5 g of aramid fiber was dissolved in 20 ml of DMF solution, and then 0.25 mL of KH-550 was added and stirred for 1 h to obtain a fiber solution;
[0059] (2) 0.456 g of PPDA was dissolved in 10 mL of DMF solution, and then 1.278 g of biphenyltetracarboxylic dianhydride (BPDA) was added and stirred to dissolve to form a precursor solution; the fiber solution in step (1) was mixed with the precursor solution and stirred for 10 min to form a mixed solution; 3.28 mL of acetic anhydride and 2.80 mL of pyridine were quickly added to the mixed solution in sequence, and after stirring for 3 min, 4.269 mL of DMF solution containing 0.019 g of 1,3,5-tris(4-aminophenoxy)benzene (TAB) was quickly added, and after stirring for 5 min, the mixture was placed in a 50°C water bath and heated for 40 min to obtain a PI / fiber wet gel;
[0060] (3) soaking the fiber / PI wet gel in step (2) in an ethanol solution containing 75% DMF by mass for 24 h, soaking it in an ethanol solution containing 25% DMF by mass for 24 h, and finally aging it in the ethanol solution for 48 h (changing it every 24 h);
[0061] (4) The aged fiber / PI wet gel is subjected to CO2 supercritical drying to obtain PI / fiber aerogel.
[0062] The stress-strain test results show that the compressive strength of PI aerogel is 1.14MPa, the shrinkage rate is 6.7%, and the porosity is 88.9%.
[0063] Example 4
[0064] (1) At 25°C, 1.5 g of polyamide fiber was dissolved in 20 ml of NMP solution, and then 0.25 mL of KH-550 was added and stirred for 1 h to obtain a fiber solution;
[0065] (2) Dissolve 0.843 g of 4,4-diaminodiphenyl ether (ODA) in 10 mL of NMP solution, then add 1.278 g of biphenyltetracarboxylic dianhydride (BPDA) and stir to dissolve to form a precursor solution; mix the fiber solution in step (1) with the precursor solution and stir for 10 min to form a mixed solution; quickly add 3.28 mL of acetic anhydride and 2.80 mL of pyridine to the mixed solution in sequence, stir for 3 min, then quickly add 4.269 mL of NMP solution containing 0.019 g of TAB, stir for 5 min, then heat in a 50°C oven for 10 min to obtain a PI / fiber wet gel;
[0066] (3) soaking the fiber / PI wet gel in step (2) in an ethanol solution containing 75% NMP by mass for 24 h, soaking it in an ethanol solution containing 25% NMP for 24 h, and finally aging it in the ethanol solution for 48 h (changing it every 24 h);
[0067] (4) The aged fiber / PI wet gel is subjected to CO2 supercritical drying to obtain PI / fiber aerogel.
[0068] The stress-strain test results show that the compressive strength of PI aerogel is 1.74MPa, the shrinkage rate is 5.2%, and the porosity is 90.4%.
[0069] Example 5
[0070] (1) At 25°C, 1.5 g of mullite fiber was dissolved in 20 ml of NMP solution, and then 0.25 mL of KH-792 was added and stirred for 1 h to obtain a fiber solution;
[0071] (2) 0.843 g of ODA was dissolved in 10 mL of NMP solution, and then 1.313 g of BTDA was added and stirred to dissolve to form a precursor solution; the fiber solution in step (1) was mixed with the precursor solution and stirred for 10 min to form a mixed solution; 5 mL of dry trifluoroacetic acid and 2.80 mL of pyridine were quickly added to the mixed solution in sequence, and after stirring for 3 min, 4.269 mL of NMP solution containing 0.019 g of TAB was quickly added, and after stirring for 3 min, the mixture was placed in a 40° C. oven and heated for 20 min to obtain a PI / fiber wet gel;
[0072] (3) soaking the fiber / PI wet gel in step (2) in an ethanol solution containing 75% NMP by mass for 24 h, soaking it in an ethanol solution containing 25% NMP for 24 h, and finally aging it in the ethanol solution for 48 h (changing it every 24 h);
[0073] (4) The aged fiber / PI wet gel is subjected to CO2 supercritical drying to obtain PI / fiber aerogel.
[0074] The stress-strain test results show that the compressive strength of PI aerogel is 1.68MPa, the shrinkage rate is 4.57%, and the porosity is 91.3%.
[0075] Example 6
[0076] (1) At 25°C, 0.5 g of aramid fiber was dissolved in 20 ml of NMP solution, and then 0.25 ml of KH-792 was added and stirred for 1 h to obtain a fiber solution;
[0077] (2) Dissolve 0.895 g of DMBZ in 10 mL of NMP solution, then add 1.278 g of BPDA and stir to dissolve to form a precursor solution; mix the fiber solution in step (1) with the precursor solution and stir for 10 min to form a mixed solution; quickly add 5.47 mL of benzoic anhydride and 2.80 mL of pyridine to the mixed solution in sequence, stir for 3 min, then quickly add 4.269 mL of NMP solution containing 0.019 g of TAB, stir for 3 min, then heat in a 40°C oven for 30 min to obtain a PI / fiber wet gel;
[0078] (3) soaking the fiber / PI wet gel in step (2) in an ethanol solution containing 75% NMP by mass for 24 h, soaking it in an ethanol solution containing 25% NMP for 24 h, and finally aging it in the ethanol solution for 48 h (changing it every 24 h);
[0079] (4) The aged fiber / PI wet gel is subjected to CO2 supercritical drying to obtain PI / fiber aerogel.
[0080] The stress-strain test results show that the compressive strength of PI aerogel is 1.02MPa, the shrinkage rate is 7.47%, and the porosity is 86.5%.
[0081] Example 7
[0082] (1) At 25°C, 0.5 g of graphite fiber was dissolved in 20 ml of NMP solution, and then 0.25 mL of KH-151 was added and stirred for 1 h to obtain a fiber solution;
[0083] (2) 0.895 g of DMBZ was dissolved in 10 mL of NMP solution, and then 1.278 g of BPDA was added and stirred to dissolve to form a precursor solution; the fiber solution in step (1) was mixed with the precursor solution and stirred for 10 min to form a mixed solution; 3.28 mL of acetic anhydride and 3.0 mL of quinoline were quickly added to the mixed solution in sequence, and after stirring for 3 min, 4.269 mL of NMP solution containing 0.019 g of TAB was quickly added, and after stirring for 3 min, the mixture was placed in a 30° C. oven and heated for 20 min to obtain a PI / fiber wet gel;
[0084] (3) soaking the fiber / PI wet gel in step (2) in an ethanol solution containing 75% NMP by mass for 24 h, soaking it in an ethanol solution containing 25% NMP for 24 h, and finally aging it in the ethanol solution for 48 h (changing it every 24 h);
[0085] (4) The aged fiber / PI wet gel is subjected to CO2 supercritical drying to obtain PI / fiber aerogel.
[0086] The stress-strain test results show that the compressive strength of PI aerogel is 0.94MPa, the shrinkage rate is 9.2%, and the porosity is 83.5%.
[0087] Comparative Example 1
[0088] The difference from Example 1 is that there is no step (1), and the other steps are exactly the same as those in Example 1.
[0089] Comparative Example 1 did not add fiber filler and was heated in an oven at 60° C. for 30 minutes. Figure 2 This is an optical picture of the prepared PI aerogel. It can be seen that the PI aerogel cannot be formed into a block, but is in powder form, with very low strength, and the compressive strength cannot be tested. The stress-strain test results show that the compressive strength of the PI aerogel in Comparative Example 1 is 0.45MPa, the shrinkage rate is 14.3%, and the porosity is 69.9%.
[0090] Comparative Example 2
[0091] The difference from Example 1 is that no coupling agent is added in step (1), and the other steps are exactly the same as Example 1.
[0092] The PI aerogel of Comparative Example 2 has a compressive strength of 0.61 MPa, a shrinkage rate of 11.3%, and a porosity of 73.5%.
[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a polyimide / fiber composite aerogel, It is characterized in that The steps include: S1: dissolving the fiber in an organic solvent, then adding a coupling agent and stirring to obtain a fiber solution; S2: dissolving the diamine in an organic solvent, then adding dianhydride and stirring to form a precursor solution; S3: mixing the fiber solution in S1 with the precursor solution in S2 to form a mixed solution; S4: adding a crosslinking agent, a catalyst and a dehydrating agent to the mixed solution in S3 in sequence to react, and obtaining a PI / fiber wet gel after drying; S5: gradient solvent replacement of the PI / fiber wet gel in S4; S6: CO2-treated PI / fiber wet gel after gradient solvent replacement in S5 2 The polyimide / fiber composite aerogel is obtained by supercritical drying.
2. The preparation method according to claim 1, It is characterized in that In step S1, the organic solvent is N-methylpyrrolidone or N,N-dimethylformamide; The fiber is molybdenum fiber, aluminum silicate fiber, graphite fiber, silica fiber, aluminum silicate ceramic fiber, carbon fiber, glass fiber, quartz fiber, basalt fiber or polycrystalline alumina fiber, aramid fiber or polyamide fiber; The coupling agent is a silane coupling agent; Preferably, the silane coupling agent is KH-550, KH-792 or KH-151.
3. The preparation method according to claim 2, It is characterized in that In step S1, the usage ratio of the organic solvent, fiber and coupling agent is (1-20) mL: (0.5-2.0) g: (0.5-0.25) mL.
4. The preparation method according to claim 1, It is characterized in that In step S2, the diamine is one or more of p-phenylenediamine, 2,2-diaminobenzidine or 4,4-diaminodiphenyl ether; The dianhydride is biphenyltetracarboxylic dianhydride or pyromellitic dianhydride; The organic solvent is N-methylpyrrolidone or N,N-dimethylformamide; Preferably, the usage ratio of the organic solvent, diamine and dianhydride is (1-20) mL: (0.5-1.0) g: (1.0-1.5) g.
5. The preparation method according to claim 1, It is characterized in that In step S4, the cross-linking agent is 1,3,5-benzenetricarboxylic acid chloride or 1,3,5-tris(4-aminophenoxy)benzene; The catalyst is pyridine, quinoline, triethylamine or isoquinoline; The dehydrating agent is acetic anhydride, benzoic anhydride, trifluoroacetic anhydride or succinic anhydride.
6. The preparation method according to claim 5, It is characterized in that In step S4, The usage ratio of the cross-linking agent, the catalyst and the dehydrating agent is (0.01-0.025) g: (2-5) mL: (3-10) mL.
7. The preparation method according to claim 1, It is characterized in that In step S5, the specific steps of the gradient solution replacement are: (1) Soaking in 70-90wt.% N-methylpyrrolidone ethanol solution for 12-48h; (2) soaking in 20-50wt.% N-methylpyrrolidone ethanol solution for 12-48h; (3) Soak in ethanol solution for 12h-48h.
8. The preparation method according to claim 1, It is characterized in that In step S6, the CO 2 The conditions for supercritical drying are: a temperature of 40 to 60°C; preferably, the temperature is 45 to 55°C; The drying pressure is 8-10Mpa; preferably, the drying pressure is 8-8.5Mpa; The drying time is 6 to 8 hours.
9. A polyimide / fiber composite aerogel prepared by the preparation method according to any one of claims 1 to 8, It is characterized in that The polyimide / fiber composite aerogel has a tensile strength of 0.9-1.87 MPa, a shrinkage rate of 4-9.2%, and a porosity of 83-91%.
10. Use of the polyimide / fiber composite aerogel according to claim 9 in thermal insulation, oil-water separation, pressure sensing, and electromagnetic protection.
Citation Information
Cited By
Synthetic fiber felt-polymer aerogel composite material and preparation and application thereof, and high-temperature-resistant emergency oil core and preparation and application thereof
CN119798991A
Activated carbon gel precursor particle with dehumidification and formaldehyde removal functions and preparation method thereof
CN121288795A
Activated carbon gel precursor particles with both dehumidification and deacetaldehyde functions and a preparation method thereof