Magnetically-driven flame-retardant polyurethane sponge for oil-water separation and preparation method thereof
By constructing a superhydrophobic surface on the sponge framework and adding magnetic nanoparticles, a magnetically driven flame-retardant polyurethane sponge with a high extrusion resistance and high adsorption capacity was prepared, which solved the problems of insufficient sponge adhesion and fire risk, and achieved efficient oil-water separation and good reusability.
Patent Information
- Application Number
- CN202410982489.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
Smart Images

Figure CN118930960A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oil-water separation materials, and specifically discloses a magnetically driven flame-retardant polyurethane sponge for oil-water separation and a preparation method thereof. Background Art
[0002] Frequent oil spills at sea have resulted in large amounts of oil leaking into the sea. In addition, oily wastewater, as a type of water pollution, is also widely present in industrial production and daily life. Oil spills cause economic losses and have serious impacts on the environment. Therefore, how to quickly, efficiently and conveniently solve this problem has attracted more and more attention from the whole society.
[0003] Traditional methods such as in-situ combustion, mechanical collection, and biodegradation are not widely used in actual oil-water separation due to their low separation efficiency and high cost of consumables. It is worth noting that physical adsorption is also used as a common means of oil-water separation, which has the advantages of high separation efficiency, low cost, and low environmental risk, and is highly recognized. At present, sponges, nanofiber aerogels, and nanofiber membranes are often used as conventional choices for physical adsorption materials. Among them, sponges have become the first choice for oil-water separation materials due to their unique three-dimensional structure, high porosity, high flexibility, and high oil absorption, and have broad application prospects in large-scale oily wastewater treatment. By constructing micro-nano structures on the sponge skeleton and modifying low surface energy substances, it becomes a superhydrophobic surface. At the same time, by utilizing its hydrophobic and lipophilic properties, effective oil selective absorption can be carried out, and oil-water separation can be achieved. However, there are also many problems. For example, the hydrophobic coating is easily separated from the sponge skeleton during the extrusion process due to the weak adhesion between the coating and the skeleton. In addition, most oils are flammable. When the sponge absorbs crude oil and organic solvents, there may be a risk of fire and explosion. Therefore, it is also crucial for the sponge to have flame retardant properties. At the same time, sponges are not easy to adsorb at multiple locations, which greatly limits their application. Summary of the invention
[0004] In order to solve the technical problems pointed out in the background technology part, the present invention provides a simple, environmentally friendly and easy-to-operate method to prepare a supermagnetically driven superhydrophobic, superoleophilic and flame-retardant polyurethane sponge which is resistant to extrusion, has high adsorption capacity, good separation efficiency and high reusability. Mobile oil absorption can be performed by magnetic drive, and no molten droplets will be generated after the sponge burns to cause secondary fire.
[0005] Specifically, the preparation method of the magnetically driven flame-retardant polyurethane sponge that can be used for efficient oil-water separation of the present invention is to add an organic ligand solution to a metal salt solution to react to obtain ZIF-67, after the product is centrifuged, washed and dried, ultrasonically dispersed in anhydrous ethanol for 30 minutes, and then nickel nitrate hexahydrate is added for reaction, and NiCo-LDH is obtained after the reaction is complete, the product is centrifuged, washed and dried, and modified by phytic acid (PA), and then the product is filtered, washed and dried, and the curing system, phytic acid-modified PA-NiCo-LDH nanoparticles and Fe3O4 particle powder are ultrasonically dispersed in n-hexane solution in turn, and the cleaned polyurethane sponge is immersed in the solution, and after ultrasonication for a period of time, it is taken out and dried to obtain a magnetically driven flame-retardant polyurethane sponge.
[0006] The organic ligand solution is a 2-methylimidazole solution with a concentration of 0.284-0.974 mol / L, and the metal salt solution is a metal cobalt salt solution with a concentration of 0.052-0.206 mol / L; the two solutions are mixed and stirred for 15 minutes, and the solvents of the two solutions are anhydrous methanol. After standing for 24 hours, centrifugation is performed, and the anhydrous methanol is washed three times, and vacuum drying is performed at 40°C;
[0007] The mass ratio of ZIF-67, nickel nitrate hexahydrate and anhydrous ethanol is 1:2.7:304. The reaction of adding nickel nitrate hexahydrate is as follows: stirring for 40 minutes, standing at 80°C for 48 hours and then centrifuging, washing with deionized water and anhydrous ethanol in turn, and drying at 40°C;
[0008] The preparation method of phytic acid modified PA-NiCo-LDH is as follows: 0.4 g NiCo-LDH and 40 mL deionized water are added into a round-bottom flask, stirred at 50° C. for 30 min to dissolve, then phytic acid solution (70%) is added, stirred for 2 h, filtered, washed and dried to obtain PA-NiCo-LDH;
[0009] The mass ratio of phytic acid solution to NiCo-LDH is 2 to 4: 5. If the amount of phytic acid is increased, the phytic acid will dissolve NiCo-LDH and PA-NiCo-LDH cannot be synthesized.
[0010] The preparation method of magnetically driven flame-retardant polyurethane sponge is as follows: the curing system is ultrasonically treated in 40 mL of n-hexane for 30 min, an appropriate amount of Fe3O4 particle powder and PA-NiCo-LDH nanoparticles are added and ultrasonically dissolved for 30 min, and then a 1 cm2 polyurethane foam that has been ultrasonically cleaned with anhydrous ethanol and deionized water is added. 3 After ultrasonic treatment for 60 minutes, the sponge was taken out, the excess immersion liquid was squeezed out with tweezers, and the sponge was placed in a 120°C oven for drying for 3 hours. After drying, the sponge was washed in n-hexane and then dried at 120°C to obtain a magnetically driven flame-retardant polyurethane sponge.
[0011] Among them, the mass ratio of the curing system, PA-NiCo-LDH and Fe3O4 is: 1.1:0.9-0.5:0.1-0.5.
[0012] The curing system uses the commonly used Dow Corning 184 product on the market, which includes a basic component (liquid A) and a curing agent (liquid B). The curing system can be obtained by ultrasonically mixing the curing agent (liquid B) and the basic component (liquid A) in a volume ratio of 1:10.
[0013] Compared with the prior art, the present invention has the following advantages:
[0014] 1. The present invention controls different mass ratios of phytic acid intercalated nickel cobalt hydrotalcite and ferroferric oxide nanoparticles to be bonded to a sponge skeleton through a curing system, wherein the phytic acid intercalated nickel cobalt hydrotalcite provides flame retardancy, and the ferroferric oxide nanoparticles provide magnetism, both of which can construct a certain roughness on the sponge skeleton, and the curing system provides low surface energy, so that the sponge achieves super hydrophobicity. These raw materials are non-toxic, non-volatile, and free of secondary pollution, and the composite sponge can be produced in batches.
[0015] 2. The hydrophobic angle of the super-hydrophobic sponge prepared by the present invention can reach 154.7°, the saturated oil absorption of n-hexane and chloroform are 33.8 g / g and 91.3 / g respectively, and the ten-time separation efficiency of n-hexane and chloroform can reach 98% and 96.5 respectively. The burning time can be extended from the original 6s to 26s, and there is no flame droplet drop during the combustion process, which will not cause secondary fire.
[0016] 3. The super-hydrophobic sponge prepared by the present invention has good reusability and environmental stability, and can basically maintain a super-hydrophobic state after multiple squeezing and soaking in solutions of different salt concentrations and pH values for 12 hours. The sponge can be moved by magnetic drive, making it more convenient to clean up oil spills. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1(a1) is a state diagram of a water drop on the cross-section of PA-NiCo-LDH / Fe3O4-PDMS-PU in Example 1 of the present invention, (a2) is a state diagram of PA-NiCo-LDH / Fe3O4-PDMS-PU in the underwater silver mirror phenomenon, (a3) are state diagrams of a water drop and an oil drop falling on the original sponge and the surface of PA-NiCo-LDH / Fe3O4-PDMS-PU in Example 1 of the present invention, respectively, (a4) is a state diagram of the original sponge in water and PA-NiCo-LDH / Fe3O4-PDMS-PU floating on water, (a5) and (a6) are state diagrams of PA-NiCo-LDH / Fe3O4-PDMS-PU before and after oil absorption by magnetic drive, and (a7) is a picture of PA-NiCo-LDH / Fe3O4-PDMS-PU adsorbed on a magnet by magnetism.
[0018] Figure 2 This is a picture of the water contact angle of the composite sponge PA-NiCo-LDH / Fe3O4-PDMS-PU in Example 1 of the present invention.
[0019] Figure 3 This is the FESEM image of the composite sponge PA-NiCo-LDH / Fe3O4-PDMS-PU of Example 1 of the present invention.
[0020] Figure 4 This is the total EDS distribution spectrum of the composite sponge PA-NiCo-LDH / Fe3O4-PDMS-PU in Example 1 of the present invention.
[0021] Figure 5 This is the selective oil absorption of chloroform and n-hexane in water by the composite sponge PA-NiCo-LDH / Fe3O4-PDMS-PU in Example 1 of the present invention.
[0022] Figure 6 This is a data graph of the saturated absorption of PA-NiCo-LDH / Fe3O4-PDMS-PU of Example 1 of the present invention to various oils / organic reagents.
[0023] Figure 7 This is the optical profile of the PA-NiCo-LDH / Fe3O4-PDMS-PU dynamic water droplet contact-detachment experiment in Example 1 of the present invention.
[0024] Figure 8 This is a time comparison chart of the combustion conditions of the original PU and PA-NiCo-LDH / Fe3O4-PDMS-PU in Example 1 of the present invention.
[0025] Fig. 9This is the hydrophobic angle data diagram of Example 1 PA-NiCo-LDH / Fe3O4-PDMS-PU of the present invention after being immersed in different salt concentrations for 12 hours.
[0026] Fig.10 This is the hydrophobic angle data diagram of Example 1 PA-NiCo-LDH / Fe3O4-PDMS-PU of the present invention after being immersed in different pH conditions for 12 hours. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with embodiments, but is not limited thereto.
[0028] 1. When the composite sponge has sufficient magnetism, try to ensure better oil absorption and flame retardancy.
[0029] 2. Oil / organic solution absorption capacity test
[0030] The oil absorption performance of the prepared composite sponge was tested by soaking it in various oils / organic solvents (such as petroleum ether, n-hexane, n-octane, heavy oil, tetrahydrofuran, benzene, toluene, pump oil, chloroform) for 5 minutes. First, the composite sponge was weighed and recorded as m1, and immersed in 25mL of oil or organic solvent for 5 minutes. When the mass absorption balance was reached, the sponge was picked out and drained (about 3 seconds) until there was no excess residual solvent dripping on the surface. The sponge was taken out and weighed as m2. The saturated absorption capacity of the sponge was represented by K, which can be calculated by the following formula:
[0031] K=(m2-m1) / m1
[0032] 3. Oil-water separation efficiency and reusability test
[0033] The reusability of the composite sponge was tested by repeated absorption-extrusion cycles. The mass of the sponge before oil absorption was recorded as m1. The sponge was immersed in oil or organic solvent at ambient temperature for 5 minutes to make the sponge saturated with absorption. The mass of the sponge at this time was recorded as m2. The saturated sponge was placed in a syringe, and the syringe was manually pushed to compress the sponge until all the oil adsorbed by the sponge was squeezed out and no oil droplets were separated. The mass of the sponge after desorption was recorded as m3, and it was placed in an oven at 60°C for drying for the next cycle. The oil-water separation efficiency was recorded as η, that is, η = (m2-m3) / (m2-m1)
[0034] 4. Environmental stability test
[0035] The composite sponge was soaked in NaCl solution with concentrations of 1%, 2%, 3%, 4%, and 5% for 12 hours, the sponge was taken out and rinsed with anhydrous ethanol, dried, and the water contact angle was measured. The composite sponge was soaked in acid-base solutions with pH = 1, 3, 5, 7, 9, 11, and 13 for 12 hours, the sponge was taken out and rinsed with anhydrous ethanol, dried, and the water contact angle was measured.
[0036] In the above embodiments 2, 3 and 4, three composite sponges are soaked and the average value of the three groups of data is taken to ensure the accuracy of the data.
[0037] Example 1
[0038] (1) 4 g of 2-methylimidazole and 3 g of cobalt nitrate hexahydrate were added to 100 mL of anhydrous methanol respectively, and stirred for 20 min to dissolve to obtain solution A and solution B. Solution B was quickly added to solution A, stirred for 15 min, and then allowed to stand for 24 h. The solution after standing was centrifuged, and then washed with anhydrous methanol for 3 times and dried in a vacuum drying oven at 40° C. to obtain ZIF-67;
[0039] (2) 0.5 g ZIF-67 was added to 200 mL anhydrous ethanol, and 1.35 g nickel nitrate hexahydrate was added after ultrasonic treatment for 30 min. The mixture was stirred for 40 min and allowed to stand at 80 °C for 48 h. After centrifugation, the mixture was washed with deionized water and anhydrous ethanol three times in sequence, and dried at 40 °C to obtain NiCo-LDH.
[0040] (3) Add 0.4 g NiCo-LDH and 40 mL deionized water into a round-bottom flask, place it in a 50 °C oil bath, stir for 30 min, add 0.32 g phytic acid solution, continue stirring for 2 h, filter, wash three times with deionized water, and dry in a 60 °C oven for 6 h to obtain PA-NiCo-LDH.
[0041] (4) Add 0.5 g of Dow Corning 184 product A liquid (polydimethylsiloxane (PDMS) with vinyl active groups) and 0.05 g of Dow Corning 184 product B liquid (polydimethylsiloxane with hydrogen groups) to 40 mL of n-hexane, and ultrasonicate for 30 min. Then, add 0.35 g of PA-NiCo-LDH and 0.15 g of Fe3O4 and ultrasonicate for 30 min. Then, add the cleaned PU and continue ultrasonicating for 1 h. Take out the sponge and put it in a 120°C oven to dry for 3 h. After drying, wash it in n-hexane and dry it again at 120°C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU.
[0042] The saturated oil absorption of the composite sponge for chloroform and n-hexane is 91.3 g / g and 31.8 g / g respectively. The burning time is delayed from the original 6 s to 26 s. The total number spectrum of element distribution is shown in Figure 4, it can be seen that the magnetism is moderate and the hydrophobic angle is 154.7°;
[0043] Example 2
[0044] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0045] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0046] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0047] (4) Add 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.45 g of PA-NiCo-LDH and 0.05 g of Fe3O4, ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU;
[0048] The saturated oil absorption of the composite sponge to chloroform and n-hexane were 97.8 g / g and 34.1 g / g, respectively, the burning time was delayed from the original 6 s to 30 s, the magnetism was weak, and the hydrophobic angle was 151.6°;
[0049] Example 3
[0050] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0051] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0052] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0053] (4) Add 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.4 g of PA-NiCo-LDH and 0.1 g of Fe3O4, ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU;
[0054] The saturated oil absorption of the composite sponge to chloroform and n-hexane were 94.4 g / g and 32.5 g / g, respectively. The burning time was delayed from the original 6 s to 28 s. The magnetism was weak and the hydrophobic angle was 152.1°.
[0055] Example 4
[0056] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0057] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0058] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0059] (4) Add 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.3 g of PA-NiCo-LDH and 0.2 g of Fe3O4, ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU;
[0060] The saturated oil absorption of the composite sponge to chloroform and n-hexane were 88.7 g / g and 29.6 g / g, respectively. The burning time was delayed from the original 6 s to 22 s. The magnetism was strong and the hydrophobic angle was 152.9°.
[0061] Example 5
[0062] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0063] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0064] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0065] (4) Add 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.25 g of PA-NiCo-LDH and 0.25 g of Fe3O4, and ultrasonicate for 30 min. Add the cleaned PU and continue ultrasonicating for 1 h. Take out the sponge and put it in a 120 ° C oven to dry for 3 h. After drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU;
[0066] The saturated oil absorption of the composite sponge to chloroform and n-hexane was 85.5 g / g and 28.2 g / g respectively, the burning time was delayed from the original 6 s to 19 s, the magnetism was strong, and the hydrophobic angle was 151.8°;
[0067] Example 6
[0068] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0069] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0070] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0071] (4) 0.3 g of Dow Corning 184 product A solution and 0.03 g of Dow Corning 184 product B solution were added to 40 mL of n-hexane, and ultrasonicated for 30 min. Then, 0.21 g of PA-NiCo-LDH and 0.09 g of Fe3O4 were added and ultrasonicated for 30 min. The cleaned PU was added and ultrasonicated for 1 h. The sponge was taken out and placed in a 120°C oven for drying for 3 h. After drying, it was washed in n-hexane and then dried at 120°C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU.
[0072] The saturated oil absorption of the composite sponge to chloroform and n-hexane were 105.5 g / g and 35.6 g / g, respectively, the burning time was delayed from the original 6 s to 14 s, the magnetism was weak, and the hydrophobic angle was 152.6°;
[0073] Example 7
[0074] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0075] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0076] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0077] (4) 0.7 g of Dow Corning 184 product A solution and 0.07 g of Dow Corning 184 product B solution were added to 40 mL of n-hexane, and ultrasonicated for 30 min. Then, 0.49 g of PA-NiCo-LDH and 0.21 g of Fe3O4 were added and ultrasonicated for 30 min. The cleaned PU was added and ultrasonicated for 1 h. The sponge was taken out and placed in a 120°C oven for drying for 3 h. After drying, it was washed in n-hexane and then dried at 120°C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU.
[0078] The saturated oil absorption of the composite sponge to chloroform and n-hexane was 82.4 g / g and 27.6 g / g respectively, the burning time was delayed from the original 6 s to 28 s, the magnetism was strong, and the hydrophobic angle was 151.4°;
[0079] Example 8
[0080] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0081] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0082] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0083] (4) Add 0.9 g of Dow Corning 184 product A solution and 0.09 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.63 g of PA-NiCo-LDH and 0.27 g of Fe3O4, ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU;
[0084] The saturated oil absorption of the composite sponge to chloroform and n-hexane was 70.3 g / g and 23.4 g / g respectively, the burning time was delayed from the original 6 s to 31 s, the magnetism was strong, and the hydrophobic angle was 147.3°;
[0085] Example 9
[0086] (1) 4 g of 2-methylimidazole and 3 g of cobalt nitrate hexahydrate were added to 50 mL of anhydrous methanol respectively, and stirred for 20 min to dissolve to obtain solution A and solution B. Solution B was quickly added to solution A, stirred for 15 min, and then allowed to stand for 24 h. The solution after standing was centrifuged, and then washed with anhydrous methanol for 3 times and dried in a vacuum drying oven at 40° C. to obtain ZIF-67;
[0087] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0088] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0089] (4) The preparation steps of PA-NiCo-LDH / Fe3O4-PDMS-PU are the same as step (4) of Example 1;
[0090] The saturated oil absorption of the composite sponge to chloroform and n-hexane was 82.6 g / g and 28.3 g / g, respectively, the burning time was delayed from the original 6 s to 20 s, the magnetism was medium, and the hydrophobic angle was 152.2°;
[0091] Example 10
[0092] (1) 4 g of 2-methylimidazole and 3 g of cobalt nitrate hexahydrate were added to 200 mL of anhydrous methanol respectively, and stirred for 20 min to dissolve to obtain solution A and solution B. Solution B was quickly added to solution A, stirred for 15 min, and then allowed to stand for 24 h. The solution after standing was centrifuged, and then washed with anhydrous methanol for 3 times and dried in a vacuum drying oven at 40° C. to obtain ZIF-67;
[0093] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0094] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0095] (4) The preparation steps of PA-NiCo-LDH / Fe3O4-PDMS-PU are the same as step (4) of Example 1;
[0096] The saturated oil absorption of the composite sponge to chloroform and n-hexane were 84.9 g / g and 29.5 g / g, respectively, the burning time was delayed from the original 6 s to 18 s, the magnetism was medium, and the hydrophobic angle was 151.9°;
[0097] Embodiment 11
[0098] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0099] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0100] (3) Add 0.4 g NiCo-LDH and 40 mL deionized water into a round-bottom flask, place it in a 50 °C oil bath, stir for 30 min, add 0.16 g phytic acid solution, continue stirring for 2 h, filter, wash three times with deionized water, and dry in a 60 °C oven for 6 h to obtain PA-NiCo-LDH.
[0101] (4) Add 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.35 g of PA-NiCo-LDH and 0.15 g of Fe3O4, ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU;
[0102] The saturated oil absorption of the composite sponge to chloroform and n-hexane were 89.7 g / g and 31.2 g / g, respectively, the burning time was delayed from the original 6 s to 22 s, the magnetism was medium, and the hydrophobic angle was 153.5°;
[0103] Example 12
[0104] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0105] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0106] (3) 0.4 g NiCo-LDH and 40 mL deionized water were added to a round-bottom flask, placed in a 50 °C oil bath, stirred for 30 min, 0.24 g phytic acid solution was added, and stirring was continued for 2 h. The mixture was filtered, washed three times with deionized water, and dried in a 60 °C oven for 6 h to obtain PA-NiCo-LDH.
[0107] (4) Add 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.35 g of PA-NiCo-LDH and 0.15 g of Fe3O4, ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / Fe3O4-PDMS-PU;
[0108] The saturated oil absorption of the composite sponge for chloroform and n-hexane were 87.9 g / g and 29.8 g / g respectively, the burning time was delayed from the original 6s to 24s, the magnetism was medium, and the hydrophobic angle was 152.8°.
[0109] Comparative Example 1
[0110] (1) 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution were added to 40 mL of n-hexane, and ultrasonicated for 30 min. Then, 0.5 g of Fe3O4 was added and ultrasonicated for 30 min. The cleaned PU was added and ultrasonicated for 1 h. The sponge was taken out and placed in a 120° C. oven for drying for 3 h. After drying, the sponge was washed in n-hexane and then dried at 120° C. to obtain Fe3O4-PDMS-PU.
[0111] The saturated oil absorption of the composite sponge to chloroform and n-hexane was 76.4 g / g and 26.2 g / g respectively, the burning time was delayed from the original 6 s to 12 s, the magnetism was strong, and the hydrophobic angle was 148.6°;
[0112] Comparative Example 2
[0113] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0114] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0115] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0116] (4) Add 0.5 g of Dow Corning 184 product A solution and 0.05 g of Dow Corning 184 product B solution to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.5 g of PA-NiCo-LDH and ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain PA-NiCo-LDH / -PDMS-PU;
[0117] The saturated oil absorption of the composite sponge to chloroform and n-hexane were 81.9 g / g and 28.4 g / g, respectively, the burning time was delayed from the original 6 s to 30 s, there was no magnetism, and the hydrophobic angle was 150.3°;
[0118] Comparative Example 3
[0119] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0120] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0121] (3) The preparation steps of PA-NiCo-LDH are the same as step (3) of Example 1;
[0122] (4) 0.35 g PA-NiCo-LDH and 0.15 g Fe3O4 were added to 40 mL n-hexane, and after ultrasonication for 30 min, the cleaned PU was added, and ultrasonication was continued for 1 h. The sponge was taken out and placed in a 120 °C oven for drying for 3 h. After drying, it was washed in n-hexane and then dried at 120 °C. PA-NiCo-LDH and Fe3O4 particles were not loaded;
[0123] The saturated oil absorption of the composite sponge to chloroform and n-hexane are 115.3 g / g and 38.4 g / g respectively, the burning time is still 6 s, there is no magnetism, and the hydrophobic angle is 128.9°.
[0124] Comparative Example 4
[0125] (1) The preparation steps of ZIF-67 are the same as step (1) of Example 1;
[0126] (2) The preparation steps of NiCo-LDH are the same as step (2) of Example 1;
[0127] (3) Add 0.5 g of Dow Corning 184 product A liquid and 0.05 g of Dow Corning 184 product B liquid to 40 mL of n-hexane, ultrasonicate for 30 min, add 0.35 g of NiCo-LDH and 0.15 g of Fe3O4, ultrasonicate for 30 min, add the cleaned PU, continue ultrasonicate for 1 h, take out the sponge and put it in a 120 ° C oven to dry for 3 h, after drying, wash it in n-hexane and then dry it at 120 ° C to obtain NiCo-LDH / Fe3O4-PDMS-PU;
[0128] The saturated oil absorption of the composite sponge for chloroform and n-hexane were 85.4 g / g and 28.7 g / g respectively, the burning time was delayed from the original 6s to 21s, the magnetism was medium, and the hydrophobic angle was 152.3°.
Claims
1. A magnetically driven flame-retardant polyurethane sponge, Features: The polyurethane sponge is prepared by mixing phytic acid-modified NiCo-LDH nanoparticles, a curing system and Fe 3 O 4 The particle powder is ultrasonically dispersed in a normal hexane solution, and then a cleaned polyurethane sponge is immersed in the solution, ultrasonically dispersed, and dried to obtain the obtained product.
2. The magnetically driven flame-retardant polyurethane sponge according to claim 1, Features: The preparation method of the phytic acid modified NiCo-LDH is as follows: 2-methylimidazole solution is added to a cobalt salt solution to react to obtain ZIF-67, after centrifugal washing and drying, ultrasonic dispersion is carried out in anhydrous ethanol, and nickel nitrate hexahydrate is continued to be added to react to obtain NiCo-LDH, the product is centrifugal washing and drying, and then a phytic acid solution is added, and after stirring, suction filtration, washing, and drying are obtained to obtain phytic acid modified NiCo-LDH, namely PA-NiCo-LDH.
3. The magnetically driven flame-retardant polyurethane sponge according to claim 2, Features: The concentration of the 2-methylimidazole solution is 0.284-0.974 mol / L, and the concentration of the cobalt salt solution is 0.052-0.206 mol / L.
4. The magnetically driven flame-retardant polyurethane sponge according to claim 2, Features: The mass ratio of the ZIF-67 to nickel nitrate hexahydrate is 1:2.
7.
5. The magnetically driven flame-retardant polyurethane sponge according to claim 2, Features: The concentration of the phytic acid solution is 70%, and the mass ratio of the phytic acid solution to NiCo-LDH is 2-4:
5.
6. The magnetically driven flame-retardant polyurethane sponge according to claim 1, Features: The curing system, PA-NiCo-LDH and Fe 3 O 4 The mass ratio is: 1.1:0.9-0.5:0.1-0.5。 7. The magnetically driven flame-retardant polyurethane sponge according to claim 1, Features: The amount of n-hexane used was 40 mL, and the curing system was ultrasonicated for 30 minutes. PA-NiCo-LDH and Fe 3 O 4 After that, ultrasonic treatment was performed for 30 min, and sponge was added for ultrasonic treatment for 60 min. The drying temperature was 120°C and the drying time was 3 h.
8. A use of the magnetically driven flame-retardant polyurethane sponge according to claim 1, Features: The magnetically driven flame-retardant polyurethane sponge is used for oil-water separation.