Environment-friendly packaging bag and preparation method thereof
By using viscose fiber and jute fiber in the packaging bags combined with water-based polyurethane and sodium carboxymethylcellulose, the environmental problems and high cost of existing difficult-to-degrade plastic packaging bags are solved, and high performance is achieved. The preparation of low-cost environmentally friendly packaging bags has improved its application prospects in daily life.
Patent Information
- Application Number
- CN202411136976.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
The existing difficult-to-degrade petroleum-based plastic packaging bags have shortcomings in environmental protection and economic applications, and the existing environmentally friendly packaging bag materials are relatively expensive and difficult to widely use.
Viscose fiber and jute fiber with a mass ratio of 1:1 were used, and 10-20% aqueous polyurethane and sodium carboxymethylcellulose were added as reinforcement materials, and the netting process, needle spraying and hot pressing molding was used. Methods: Prepare environmentally friendly packaging bags to improve the mechanical properties and degradability of the materials.
It has achieved improvements in the mechanical strength and water resistance of environmentally friendly packaging bags, reduced the cost of raw materials, and has good market prospects and economic application potential.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of packaging materials, and in particular to an environmentally friendly packaging bag and a preparation method thereof. Background Art
[0002] Traditional plastic packaging bags refer to packaging bags made of high molecular compounds such as polystyrene, polypropylene, and polyvinyl chloride, which are difficult to degrade and have a long degradation cycle. Developing environmentally friendly materials to replace petroleum-based plastics has become a focus of attention.
[0003] The existing invention patent CN 111674099 A discloses an environmentally friendly packaging bag and a preparation method thereof. The preparation method of the environmentally friendly packaging bag of the invention has the characteristics of simple process flow, high production efficiency and low production cost, but it does not change the material in essence. The function of achieving environmental protection lies in the use of paper bags, and the paper bag body cannot be applied to many fields in daily life; currently, degradable packaging materials include polylactic acid, which is green and pollution-free and has become one of the most actively developed and fastest-growing biodegradable polymer materials in recent years, but its cost is relatively high, currently on the market at about 50,000 / t, and the application cost is too high.
[0004] Therefore, we consider designing a bag that can replace the existing difficult-to-degrade petroleum-based plastic bags, so that it has better degradability and good material mechanical properties, so that it has better economic application prospects; in view of this, we propose an environmentally friendly packaging bag and its preparation method. Summary of the invention
[0005] The purpose of the present invention is to solve the deficiencies mentioned in the above background technology and to provide an environmentally friendly packaging bag and a preparation method thereof.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] An environmentally friendly packaging bag comprises viscose fiber and jute fiber in a mass ratio of 1:1, and also comprises a reinforcing material accounting for 10-20% of the total mass of the viscose fiber and the jute fiber.
[0008] Preferably, the reinforcing material comprises aqueous polyurethane and sodium carboxymethyl cellulose in a mass ratio of 1-3:1.
[0009] Preferably, the surface density of the environmentally friendly packaging bag is 90-130g / m 2 .
[0010] Preferably, the environmentally friendly packaging bag has a thickness of 5-60 threads.
[0011] A method for preparing an environmentally friendly packaging bag, the specific steps of the preparation method are:
[0012] Step 1: Web-forming process: viscose fiber and jute fiber are mixed in proportion, opened and fed into a carding machine, and a fiber web is obtained after 2-3 cardings by the carding machine;
[0013] Step 2: preparing a reinforcing liquid, weighing water-based polyurethane and sodium carboxymethyl cellulose according to a proportion, dissolving the water-based polyurethane and sodium carboxymethyl cellulose in water to obtain a reinforcing liquid;
[0014] Step 3: Needle punching and spraying: feed the fiber web into the needle punching machine for needle punching reinforcement treatment, and simultaneously spray the reinforcing liquid prepared in step 2 onto the fiber web;
[0015] Step 4: Pre-drying: drying the fiber web in step 3 at 60-80°C for 2-6 hours;
[0016] Step 5: hot pressing, moving the dried fiber web to a flat vulcanizer for hot pressing to obtain an environmentally friendly membrane structure;
[0017] Step 6: Use the environmentally friendly film structure, roll it into a tube, cut it according to the size of the packaging bag, and press the edge to complete the bag making.
[0018] Preferably, in step 2, the solid-liquid ratio of the total mass of the aqueous polyurethane and sodium carboxymethyl cellulose to water is set to 1-2:10.
[0019] Preferably, in step 3, the needle punching density of the needle punching machine is set to 180-260 needles / cm 2 The number of acupuncture points is 1-3.
[0020] Preferably, the hot pressing molding is performed at a hot pressing temperature of 150-180° C., a hot pressing time of 30-60 s, and a hot pressing pressure of 4-6 MPa.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The environmentally friendly packaging bag and its preparation method creatively use water-based polyurethane and sodium carboxymethyl cellulose to improve the mechanical strength and water resistance of viscose fiber and jute fiber bags;
[0023] 2. All raw material components are degradable, and green and environmentally friendly security bags can be produced. The cost of raw materials is not high, and it has a good market prospect;
[0024] 3. The preparation method can fully mix the reinforcing liquid into the fiber web made of viscose fiber and jute fiber, which is beneficial to improving the mechanical properties. The preparation method is simple and suitable for mass production. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. In the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.
[0026] The present invention describes the above technical solution in detail through the following embodiments:
[0027] Example 1
[0028] The invention discloses an environmentally friendly packaging bag, which comprises viscose fiber and jute fiber in a mass ratio of 1:1, and also comprises a reinforcing material accounting for 20% of the total mass of the viscose fiber and the jute fiber.
[0029] The preparation method of the environmentally friendly packaging bag in this embodiment has the following specific steps:
[0030] Step 1: web forming process. In this embodiment, the raw material jute fiber has a fiber linear density of 32.3 dtex, a breaking elongation of 1.89%, and a breaking strength of 3.35 cN / dtex; the viscose fiber has a fiber linear density of 2 dtex, a breaking elongation of 15.64, and a breaking strength of 2.41 cN / dtex; the viscose fiber and the jute fiber are mixed in equal proportions, and after opening, they are fed into a FZS-600 single cylinder double doffer carding machine to obtain a fiber web after three cardings;
[0031] Step 2: preparing a reinforcing liquid, weighing a reinforcing material accounting for 20% of the total mass of the viscose fiber and the jute fiber, wherein the reinforcing material comprises an aqueous polyurethane and sodium carboxymethyl cellulose in a mass ratio of 3:1, dissolving the aqueous polyurethane and sodium carboxymethyl cellulose in water, and controlling the solid-liquid ratio to be 1:10 to obtain a reinforcing liquid;
[0032] Step 3: Needle punching spraying: feed the fiber web into the FZZ-1000 main needle punching machine for needle punching reinforcement treatment, and spray the reinforcement liquid configured in step 2 evenly on the fiber web at the same time. Set the needle punching density of the needle punching machine to 220 needles / cm 2 , the number of acupuncture points is 3;
[0033] Step 4: Pre-drying: drying the fiber web in step 3 at 60°C for 6 hours;
[0034] Step 5: Hot pressing: the dried fiber web is moved to the XLB-400×400×2 flat vulcanizer for hot pressing. The hot pressing temperature is set to 165°C, the hot pressing time is 50s, and the hot pressing pressure is 5MPa. The surface density is 110g / m 2, the environmentally friendly film structure has a thickness of 40 threads. It needs to be explained that the thickness of the bag body is 100 threads, which is equal to 1 mm, that is, the environmentally friendly film structure of this embodiment is 0.4 mm thick; the environmentally friendly film structure is used, rolled into a tube, and cut and pressed according to the size of the packaging bag to complete the bag making.
[0035] Example 2
[0036] The difference between this embodiment and embodiment 1 is limited to that in this embodiment, a reinforcing material accounting for 10% of the total mass of viscose fiber and jute fiber is provided, and other conditions are the same.
[0037] Example 3
[0038] The difference between this embodiment and embodiment 1 is limited to that the mass ratio of waterborne polyurethane to sodium carboxymethyl cellulose in this embodiment is 1:1, and other conditions are the same.
[0039] Example 4
[0040] The difference between this embodiment and embodiment 1 is limited to that the mass ratio of waterborne polyurethane to sodium carboxymethyl cellulose in this embodiment is 2:1, and other conditions are the same.
[0041] Example 5
[0042] The difference between this embodiment and embodiment 1 is limited to: in this embodiment, the needling spraying step is implemented in steps, first puncturing and then spraying the reinforcing liquid, and other conditions are the same.
[0043] Example 6
[0044] The difference between this embodiment and embodiment 1 is limited to that the solid-liquid ratio of the total mass of waterborne polyurethane and sodium carboxymethyl cellulose to water in this embodiment is 1:5, and other conditions are the same.
[0045] Comparative Example 1
[0046] The difference between this comparative example and Example 1 is only that in this comparative example, a reinforcing material accounting for 2% of the total mass of the viscose fiber and the jute fiber is provided, and other conditions are the same.
[0047] Comparative Example 2
[0048] The difference between this comparative example and Example 1 is only that in this comparative example, a reinforcing material accounting for 25% of the total mass of the viscose fiber and the jute fiber is provided, and other conditions are the same.
[0049] Comparative Example 3
[0050] The difference between this comparative example and Example 1 is only that the mass ratio of waterborne polyurethane to sodium carboxymethyl cellulose in this comparative example is 4:1, and other conditions are the same.
[0051] Comparative Example 4
[0052] The difference between this comparative example and Example 1 is only that the mass ratio of waterborne polyurethane to sodium carboxymethyl cellulose in this comparative example is 1:2, and other conditions are the same.
[0053] Comparative Example 5
[0054] The difference between this comparative example and Example 1 is limited to that the solid-liquid ratio of the total mass of aqueous polyurethane and sodium carboxymethyl cellulose to water in this comparative example is 0.5:10, and other conditions are the same.
[0055] Comparative Example 6
[0056] The difference between this comparative example and Example 1 is limited to that the solid-liquid ratio of the total mass of aqueous polyurethane and sodium carboxymethyl cellulose to water in this comparative example is 3:10, and other conditions are the same.
[0057] (1) According to Examples 1-6 and Comparative Examples 1-6, each sample was prepared separately without bagging, and the environmentally friendly membrane structure prepared in step 5 was tested for its mechanical properties;
[0058] Test standard: Reference standard GB / T24218.3-2010 "Test methods for textile nonwovens Part 3: Determination of breaking strength and breaking elongation (strip method)"; Set the strip width to 50mm±0.5mm, the gauge length to 100mm, and the stretching speed to 100mm / min; Test instrument: HD026N multifunctional fabric strength tester; Specific parameters are as follows:
[0059]
[0060]
[0061] According to the above table, Example 1-2 and Comparative Example 1-2, when the reinforcing material decreases, the mechanical properties will be attenuated, but excessive reinforcing material will not lead to a significant increase in the mechanical properties of the material, but will lead to a decrease in the corresponding elongation at break, that is, the tensile toughness of the material is reduced. Therefore, from the perspective of production economy, the excessive embodiment is not adopted;
[0062] According to Example 1, Example 3-4, and Comparative Example 3-4, it can be seen that the mass ratio of waterborne polyurethane and sodium carboxymethyl cellulose affects the mechanical properties of the material. When the amount of sodium carboxymethyl cellulose increases, its mechanical properties can be significantly improved, but its elongation at break will also decrease;
[0063] When the amount of sodium carboxymethyl cellulose is lower than the patent range, the material performance shows obvious attenuation, but when the amount of sodium carboxymethyl cellulose is too large, the mechanical properties of the material show a sudden drop, that is, the breaking strength and elongation show a sudden attenuation. Considering that excessive sodium carboxymethyl cellulose leads to excessive viscosity of the material, turning from toughness to brittleness, the comparative process is not advisable;
[0064] From the data of Example 1, Example 6, and Comparative Examples 5-6, it can be seen that the solid-liquid ratio of the total mass of waterborne polyurethane and sodium carboxymethyl cellulose to water affects the mechanical properties of the material. The material properties tend to be stable when the solid content is increased. However, it is found in the process that the lower the solid content, the easier it is to spray evenly and the easier it is to operate. However, if the solid content is low, that is, the amount of water dissolved in water is large, the mechanical properties of the material will be significantly attenuated.
[0065] It can be seen from the data of Example 1 and Example 5 that synchronous needle puncture spraying is beneficial to improving the mechanical properties of the material. Considering that puncture can enable the spray liquid to penetrate into the interior of the fiber, the overall material performance is improved.
[0066] (2) Select samples from Example 1, Example 3, Example 4, and Comparative Example 4, respectively, and immerse them in water for 1 hour and then take them out, and test their mechanical properties again, and test their strength retention rate;
[0067] Strength retention rate = mechanical strength after immersion in water / mechanical strength before immersion in water × 100%
[0068] The data is as follows:
[0069]
[0070] The strength retention rate can be measured based on the breaking strength data before and after immersion in water. The ratio of water-based polyurethane to sodium carboxymethyl cellulose also affects the water resistance of the material. Within the scope of the patent, the higher the proportion of water-based polyurethane, the better the water resistance and the higher the strength retention rate. The higher the strength retention rate, the better the water resistance. If the proportion of water-based polyurethane is too small, the water resistance will be seriously lacking. If the proportion of water-based polyurethane is too large, the data in the above table has already reflected this, which has an impact on the mechanical properties.
[0071] In addition, it should be explained that the raw materials in this patent are all environmentally friendly. Jute fiber and viscose fiber have excellent degradability and can be self-degraded in the natural environment through the action of light, heat and microorganisms. The creative water-based polyurethane and sodium carboxymethyl cellulose, wherein the water-based polyurethane uses water as a solvent, has the performance characteristics of being pollution-free, safe and environmentally friendly, waterproof and biodegradable. Sodium carboxymethyl cellulose is a cellulose ether made from natural cellulose, which has high degradation performance, and its aqueous solution has good thickening, adhesion, film-forming and dispersion properties. Therefore, the raw materials of the packaging bag components are all degradable and are environmentally friendly materials. The cost of water-based polyurethane and sodium carboxymethyl cellulose is about RMB 6,000-12,000 / t, which has better market prospects than the existing polylactic acid.
[0072] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. An environmentally friendly packaging bag, characterized in that: The environmentally friendly packaging bag comprises viscose fiber and jute fiber in a mass ratio of 1:1, and also comprises reinforcing material accounting for 10-20% of the total mass of the viscose fiber and the jute fiber.
2. The environmentally friendly packaging bag according to claim 1, characterized in that: The reinforcing material comprises aqueous polyurethane and sodium carboxymethyl cellulose in a mass ratio of 1-3:
1.
3. The environmentally friendly packaging bag according to claim 1, characterized in that: The surface density of the environmentally friendly packaging bag is 90-130g / m 2 .
4. The environmentally friendly packaging bag according to claim 3, characterized in that: The thickness of the environmentally friendly packaging bag is 5-60 threads.
5. A method for preparing an environmentally friendly packaging bag, applicable to the environmentally friendly packaging bag according to any one of claims 1 to 4, characterized in that: The specific steps of the preparation method are: Step 1: Web-forming process: viscose fiber and jute fiber are mixed in proportion, opened and fed into a carding machine, and a fiber web is obtained after 2-3 cardings by the carding machine; Step 2: preparing a reinforcing liquid, weighing water-based polyurethane and sodium carboxymethyl cellulose according to a proportion, dissolving the water-based polyurethane and sodium carboxymethyl cellulose in water to obtain a reinforcing liquid; Step 3: Needle punching and spraying: feed the fiber web into the needle punching machine for needle punching reinforcement treatment, and simultaneously spray the reinforcing liquid prepared in step 2 onto the fiber web; Step 4: Pre-drying: drying the fiber web in step 3 at 60-80°C for 2-6 hours; Step 5: hot pressing, moving the dried fiber web to a flat vulcanizer for hot pressing to obtain an environmentally friendly membrane structure; Step 6: Use the environmentally friendly film structure, roll it into a tube, cut it according to the size of the packaging bag, and press the edge to complete the bag making.
6. The method for preparing the environmentally friendly packaging bag according to claim 5, characterized in that: In the step 2, the solid-liquid ratio of the total mass of the aqueous polyurethane and sodium carboxymethyl cellulose to water is set to 1-2:
10.
7. The method for preparing an environmentally friendly packaging bag according to claim 5, characterized in that: In step 3, the needle punching density of the needle punching machine is set to 180-260 needles / cm 2 The number of acupuncture points is 1-3.
8. The method for preparing an environmentally friendly packaging bag according to claim 5, characterized in that: The hot pressing molding is performed at a hot pressing temperature of 150-180° C., a hot pressing time of 30-60 seconds, and a hot pressing pressure of 4-6 MPa.