Degradable composite material, preparation method thereof and application of degradable composite material in chopsticks
Through the composite technology of starch, polyβ-hydroxybutyrate and other materials, degradable chopstick materials with excellent mechanical properties and high degradation rate were prepared, which solved the shortcomings of existing chopstick materials on the environment and performance, and achieved biodegradation and The goal of environmental protection.
Patent Information
- Application Number
- CN202411147914.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
Existing chopstick materials such as wood, bamboo and plastics have ecological and environmental problems. Starch chopsticks have poor mechanical properties and low antibacterial properties, making them difficult to meet biodegradation and environmental protection requirements.
Composite materials such as starch, polyβ-hydroxybutyrate, composite microspheres, activated bamboo fibers and polyamides are used to form a degradable composite material with excellent mechanical properties and antibacterial properties through low temperature compression and ultrasonic treatment. Prepare chopsticks.
The biodegradability, mechanical properties and antibacterial properties of chopsticks have been improved, with a degradation rate of more than 90%, reducing the consumption of forest resources and having high economic and social benefits.
Smart Images

Figure CN118930984A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of degradable tableware, and in particular to a degradable composite material and a preparation method thereof and application in chopsticks. Background Art
[0002] At present, in the chopstick industry, most of the focus at home and abroad is on the research of wood production technology. Most of the chopsticks on the market are made of wood or bamboo. Chopsticks made of bamboo and wood are not only easy to breed bacteria, but also require a large amount of natural materials such as wood and bamboo to produce chopsticks, leading to problems such as reduced forest coverage and environmental deterioration. Therefore, the industry is actively seeking new ways out for chopsticks.
[0003] At present, there are chopsticks made of starch as the main raw material, but such chopsticks have poor mechanical properties and low antibacterial properties, which easily breed bacteria, limiting the scope of application of chopsticks. Nowadays, plastics are used to produce disposable chopsticks instead of wood and bamboo, but plastic chopsticks will cause pollution after being discarded and are difficult to degrade.
[0004] As people's awareness of protecting forest resources and environmental protection increases, some disposable chopsticks made of new materials have appeared. The development of degradable plastics for chopsticks is of great significance to protecting the environment. Plastic products used for chopsticks not only need to have good biodegradability, but also need to have good mechanical properties and antibacterial properties, which needs to be urgently solved. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a degradable composite material and a preparation method thereof and application in chopsticks.
[0006] A degradable composite material, whose raw materials include, by weight: 50-100 parts of starch, 10-20 parts of poly-β-hydroxybutyrate, 5-15 parts of composite microspheres, 1-3 parts of polyamidoamine, 5-10 parts of activated bamboo fibers, 0.1-1 parts of a crosslinking agent, and 1-2 parts of a plasticizer.
[0007] The raw materials of the composite microspheres include, by mass, 20-40 parts of vegetable oil, 1-3 parts of lecithin, 1-2 parts of emulsifier, 1-2 parts of complex enzyme, 1-2 parts of glycerol, 1-2 parts of gelatin, 1-2 parts of chitosan, and 8-20 parts of ammonium sulfate. The activated bamboo fiber is obtained by depositing nano titanium dioxide on the bamboo fiber after alkali washing.
[0008] Preferably, the polyamidoamine has a generation number of 4.0-6.0.
[0009] Preferably, the cross-linking agent comprises: sodium hexametaphosphate and sodium polyphosphate; wherein the mass ratio of sodium hexametaphosphate to sodium polyphosphate is 1:0.1-1.
[0010] Preferably, the plasticizer is calcium stearate and / or zinc stearate.
[0011] Preferably, the vegetable oil is at least one of soybean oil, palm oil, corn oil, peanut oil and rapeseed oil.
[0012] Preferably, the emulsifier is at least one of succinic acid monoglyceride, polyglycerol fatty acid ester, and sucrose fatty acid ester.
[0013] Preferably, the complex enzyme comprises amylase, cellulase and protease; wherein the enzymatic activity of the amylase is 10000-20000 U / g, the enzymatic activity of the cellulase is 3000-4000 U / g, and the enzymatic activity of the protease is 6000-9000 U / g.
[0014] Preferably, the composite microspheres are prepared by the following specific operations: adding lecithin and emulsifier to vegetable oil and stirring evenly to obtain pretreated vegetable oil; adding complex enzyme, glycerol, gelatin, and chitosan to acetic acid aqueous solution and stirring evenly, adding dropwise to the stirred pretreated vegetable oil, stirring for 10-20 minutes after the addition is complete, adding ammonium sulfate solution and stirring for 1-2 hours, centrifuging, and freeze-drying.
[0015] Preferably, the activated bamboo fiber is prepared by the following specific operation: the bamboo fiber is crushed and sieved, sent into a sodium hydroxide solution to soak for 10-20 hours, filtered, washed, dried, added to water, tetrabutyl titanate is added thereto and ultrasonically treated for 10-30 minutes, the pH value of the system is adjusted to 8-9, the ultrasonic treatment is continued for 1-2 hours, centrifuged, washed, and dried.
[0016] Preferably, the mass ratio of bamboo fiber to tetrabutyl titanate is 5-10:1-2.
[0017] Preferably, the ultrasound frequency is 10-16 kHz.
[0018] The preparation method of the above-mentioned degradable composite material comprises the following steps: starch, poly-β-hydroxybutyrate, composite microspheres and polyamide amine are mixed evenly, activated bamboo fiber, crosslinking agent and plasticizer are added and stirring is continued for 10-20 minutes, the mixture is put into a mold, and pressed at a low temperature of 50-60°C for 1-5 minutes, with a pressing pressure of 1-3MPa.
[0019] Application of the above-mentioned degradable composite material in chopsticks.
[0020] Beneficial effects:
[0021] The invention adopts starch and poly-β-hydroxybutyrate compound, has excellent biodegradability and thermoplastic processability, and combined with the effect of activated bamboo fiber, the product has excellent toughness, and good antibacterial and water-resistant properties.
[0022] Since lecithin has a hydrophilic head composed of substituents connected to phosphate and a hydrophobic tail composed of fatty acid chains, it has good coating properties for complex enzymes. When combined with glycerol and gelatin, it forms a network of hydrogen bonds when the solvent evaporates, which significantly enhances the coating effect on the complex enzyme. However, its stability is poor and it is very easy to break in subsequent processes, resulting in the complex enzyme being unable to function normally.
[0023] The present invention adopts chitosan in combination with glycerol and gelatin. The chitosan molecule contains a large number of hydroxyl groups and amino groups, which can form stable hydrogen bonds with glycerol and gelatin to enhance the coating effect of the complex enzyme, and can also form microspheres through ammonium sulfate precipitation. The microspheres have a compact structure and excellent stability, and can effectively release the complex enzyme contained in the chopsticks during the degradation process. The test shows that the degradation rate of the product can reach more than 90% after only 60 days of degradation.
[0024] The present invention uses composite microspheres compounded with starch and poly-β-hydroxybutyrate, and adopts a low-temperature processing method, which can not only provide a good environment for the composite enzyme, effectively avoid direct contact between the composite enzyme and the material, reduce damage to the composite enzyme, but also maintain high activity under high humidity, effectively adjust the degradation rate of the material, and thus achieve controllable degradation. The present invention further adds polyamidoamine containing a large number of active terminal amino groups, which can be more easily combined with the terminal carboxylic acid on the lecithin structure, and its special dendritic structure is entangled with starch and poly-β-hydroxybutyrate molecular chain structure, so that the product has high static bending strength, no damage when falling, and excellent mechanical properties.
[0025] The invention meets various performance standards, is convenient, green and environmentally friendly, saves wood consumption, and has higher economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a comparison chart of the tensile strength and elongation at break of the degradable composite materials obtained in Example 5 and Comparative Examples 1-2.
[0027] Figure 2 It is a comparison chart of the bending strength and maximum drop height of the degradable composite materials obtained in Example 5 and Comparative Examples 1-2.
[0028] Figure 3 The degradation curves of chopsticks made from the degradable composite materials obtained in Example 5 and Comparative Examples 1-2 are shown. DETAILED DESCRIPTION
[0029] The present invention will be further explained below in conjunction with specific embodiments.
[0030] Example 1
[0031] A degradable composite material, the raw materials of which include: 50kg starch, 10kg poly-β-hydroxybutyrate, 5kg composite microspheres, 1kg 4.0 generation polyamidoamine, 5kg activated bamboo fiber, 0.1kg crosslinking agent, and 1kg calcium stearate. The crosslinking agent is obtained by mixing sodium hexametaphosphate and sodium polyphosphate in a mass ratio of 1:0.1.
[0032] The raw materials of the composite microspheres include: 20kg soybean oil, 1kg lecithin, 1kg succinic acid monoglyceride, 1kg composite enzyme, 1kg glycerol, 1kg gelatin, 1kg chitosan, and 8kg ammonium sulfate. The composite enzyme includes: amylase with an enzyme activity of 10,000U / g, cellulase with an enzyme activity of 3,000U / g, and protease with an enzyme activity of 6,000U / g.
[0033] The composite microspheres were prepared by the following specific operations: adding lecithin and succinic acid monoglyceride to soybean oil and stirring evenly to obtain pretreated soybean oil; adding complex enzyme, glycerol, gelatin and chitosan to 5 kg of 0.1 mol / L acetic acid aqueous solution and stirring evenly, and then dropping them into the stirred pretreated soybean oil at a stirring speed of 1500 r / min. After the dropping was complete, stirring for 10 minutes, adding a 40% ammonium sulfate solution by mass and stirring for 1 hour, centrifuging and freeze-drying.
[0034] The activated bamboo fiber was prepared by the following specific operation: 5 kg of bamboo fiber was crushed and passed through a 60-mesh sieve, and was sent to 20 kg of a 10.5 mol / L sodium hydroxide solution and soaked for 10 hours, filtered, washed with deionized water, dried, added to 20 kg of water, 1 kg of tetrabutyl titanate was added thereto, and ultrasonic treatment was performed for 10 minutes at an ultrasonic frequency of 10 kHz. The pH value of the system was adjusted to 8-9 with a 0.5 mol / L sodium hydroxide solution, and the ultrasonic treatment was continued for 1 hour, centrifuged, washed with deionized water, and dried.
[0035] The preparation method of the above-mentioned degradable composite material includes the following steps: starch, poly-β-hydroxybutyrate, composite microspheres, and polyamide amine are mixed evenly, activated bamboo fiber, crosslinking agent, and calcium stearate are added and stirring is continued for 10 minutes, the mixture is put into a mold, pressed at a low temperature of 50°C for 1 minute with a pressing pressure of 1MPa, taken out after cooling, coated with a protective film, and sterilized with ultraviolet light.
[0036] Example 2
[0037] A degradable composite material, the raw materials of which include: 100kg starch, 20kg poly-β-hydroxybutyrate, 15kg composite microspheres, 3kg 6.0 generation polyamidoamine, 10kg activated bamboo fiber, 1kg crosslinking agent, and 2kg calcium stearate. The crosslinking agent is obtained by mixing sodium hexametaphosphate and sodium polyphosphate in a mass ratio of 1:1.
[0038] The raw materials of the composite microspheres include: 40kg peanut oil, 3kg lecithin, 2kg polyglycerol fatty acid ester, 2kg composite enzyme, 2kg glycerol, 2kg gelatin, 2kg chitosan, and 20kg ammonium sulfate. The composite enzyme includes: amylase with an enzyme activity of 20,000U / g, cellulase with an enzyme activity of 4,000U / g, and protease with an enzyme activity of 9,000U / g.
[0039] The composite microspheres are prepared by the following specific operations: adding lecithin and polyglycerol fatty acid ester to peanut oil and stirring evenly to obtain pretreated peanut oil; adding complex enzyme, glycerol, gelatin and chitosan to 10 kg of 0.2 mol / L acetic acid aqueous solution and stirring evenly, adding dropwise to the pretreated peanut oil in a stirring state at a stirring speed of 2000 r / min, stirring for 20 minutes after the dropping is complete, adding a 50% by mass ammonium sulfate solution and stirring for 2 hours, centrifuging and freeze-drying.
[0040] The activated bamboo fiber was prepared by the following specific operation: 10 kg of bamboo fiber was crushed and passed through a 60-mesh sieve, and then placed in 40 kg of a 12 mol / L sodium hydroxide solution and soaked for 20 hours, filtered, washed with deionized water, dried, added to 40 kg of water, 2 kg of tetrabutyl titanate was added thereto, and ultrasonic treatment was performed for 30 minutes at an ultrasonic frequency of 16 kHz. A 1.5 mol / L sodium hydroxide solution was used to adjust the pH value of the system to 8-9, and the ultrasonic treatment was continued for 2 hours, centrifuged, washed with deionized water, and dried.
[0041] The preparation method of the above-mentioned degradable composite material comprises the following steps: starch, poly-β-hydroxybutyrate, composite microspheres and polyamide amine are mixed evenly, activated bamboo fiber, crosslinking agent and calcium stearate are added and stirring is continued for 20 minutes, the mixture is put into a mold, pressed at a low temperature of 60°C for 5 minutes with a pressing pressure of 3MPa, taken out after cooling, coated with a protective film, and sterilized with ultraviolet light.
[0042] Example 3
[0043] A degradable composite material, the raw materials of which include: 70kg starch, 18kg poly-β-hydroxybutyrate, 8kg composite microspheres, 2.5kg 5.0 generation polyamidoamine, 7kg activated bamboo fiber, 0.7kg crosslinking agent, and 1.3kg zinc stearate. The crosslinking agent is obtained by mixing sodium hexametaphosphate and sodium polyphosphate in a mass ratio of 1:0.7.
[0044] The raw materials of the composite microspheres include: 25kg rapeseed oil, 2.5kg lecithin, 1.3kg sucrose fatty acid ester, 1.8kg composite enzyme, 1.3kg glycerol, 1.8kg gelatin, 1.4kg chitosan, and 16kg ammonium sulfate. The composite enzyme includes: amylase with an enzyme activity of 12000U / g, cellulase with an enzyme activity of 3700U / g, and protease with an enzyme activity of 7000U / g.
[0045] The composite microspheres are prepared by the following specific operations: adding lecithin and sucrose fatty acid ester to rapeseed oil and stirring evenly to obtain pretreated rapeseed oil; adding complex enzyme, glycerol, gelatin and chitosan to 9kg of 0.15mol / L acetic acid aqueous solution and stirring evenly, adding dropwise to the pretreated rapeseed oil in a stirring state at a stirring speed of 1700r / min, stirring for 17min after the dropping is complete, adding ammonium sulfate solution with a mass fraction of 42% and stirring for 100min, centrifuging and freeze-drying.
[0046] The activated bamboo fiber was prepared by the following specific operation: 7 kg of bamboo fiber was crushed and passed through a 60-mesh sieve, and was sent to 35 kg of 11 mol / L sodium hydroxide solution for immersion for 18 hours, filtered, washed with deionized water, dried, added to 25 kg of water, 1.7 kg of tetrabutyl titanate was added thereto, and ultrasonic treatment was performed for 15 minutes at an ultrasonic frequency of 13 kHz. The pH value of the system was adjusted to 8-9 with a 0.8 mol / L sodium hydroxide solution, and the ultrasonic treatment was continued for 100 minutes, centrifuged, washed with deionized water, and dried.
[0047] The preparation method of the above-mentioned degradable composite material includes the following steps: evenly mixing starch, poly-β-hydroxybutyrate, composite microspheres, and polyamide amine, adding activated bamboo fiber, crosslinking agent, and zinc stearate and continuing to stir for 12 minutes, putting into a mold, pressing at a low temperature of 58°C for 2 minutes, the pressing pressure is 2.5MPa, taking out after cooling, spraying a protective film, and ultraviolet sterilization.
[0048] Example 4
[0049] A degradable composite material, the raw materials of which include: 90kg starch, 12kg poly-β-hydroxybutyrate, 12kg composite microspheres, 1.5kg 5.0 generation polyamidoamine, 9kg activated bamboo fiber, 0.3kg crosslinking agent, and 1.7kg zinc stearate. The crosslinking agent is obtained by mixing sodium hexametaphosphate and sodium polyphosphate in a mass ratio of 1:0.3.
[0050] The raw materials of the composite microspheres include: 35kg corn oil, 1.5kg lecithin, 1.7kg polyglycerol fatty acid ester, 1.2kg composite enzyme, 1.7kg glycerol, 1.2kg gelatin, 1.8kg chitosan, and 12kg ammonium sulfate. The composite enzyme includes: amylase with an enzyme activity of 18000U / g, cellulase with an enzyme activity of 3300U / g, and protease with an enzyme activity of 8000U / g.
[0051] The composite microspheres are prepared by the following specific operations: adding lecithin and polyglycerol fatty acid ester to corn oil and stirring evenly to obtain pretreated corn oil; adding complex enzyme, glycerol, gelatin and chitosan to 7kg of 0.15mol / L acetic acid aqueous solution and stirring evenly, adding dropwise to the pretreated corn oil in a stirring state at a stirring speed of 1900r / min, stirring for 13min after the dropping is complete, adding ammonium sulfate solution with a mass fraction of 48% and stirring for 80min, centrifuging and freeze-drying.
[0052] The activated bamboo fiber was prepared by the following specific operation: 9 kg of bamboo fiber was crushed and passed through a 60-mesh sieve, and sent to 25 kg of 11.5 mol / L sodium hydroxide solution for soaking for 12 hours, filtered, washed with deionized water, dried, added to 35 kg of water, 1.3 kg of tetrabutyl titanate was added thereto, and ultrasonic treatment was performed for 25 minutes at an ultrasonic frequency of 11 kHz. The pH value of the system was adjusted to 8-9 with a sodium hydroxide solution with a concentration of 1.2 mol / L, and the ultrasonic treatment was continued for 80 minutes, centrifuged, washed with deionized water, and dried.
[0053] The preparation method of the above-mentioned degradable composite material includes the following steps: evenly mixing starch, poly-β-hydroxybutyrate, composite microspheres, and polyamide amine, adding activated bamboo fiber, a crosslinking agent, and zinc stearate and continuing to stir for 18 minutes, putting into a mold, pressing at a low temperature of 52°C for 4 minutes, the pressing pressure is 1.5MPa, taking out after cooling, spraying a protective film, and sterilizing with ultraviolet light.
[0054] Example 5
[0055] A degradable composite material, the raw materials of which include: 80kg starch, 15kg poly-β-hydroxybutyrate, 10kg composite microspheres, 2kg 5.0 generation polyamidoamine, 8kg activated bamboo fiber, 0.5kg crosslinking agent, and 1.5kg zinc stearate. The crosslinking agent is obtained by mixing sodium hexametaphosphate and sodium polyphosphate in a mass ratio of 1:0.5.
[0056] The raw materials of the composite microspheres include: 30kg palm oil, 2kg lecithin, 1.5kg succinic acid monoglyceride, 1.5kg composite enzyme, 1.5kg glycerol, 1.5kg gelatin, 1.6kg chitosan, and 14kg ammonium sulfate. The composite enzyme includes: amylase with an enzyme activity of 15000U / g, cellulase with an enzyme activity of 3500U / g, and protease with an enzyme activity of 7500U / g.
[0057] The composite microspheres are prepared by the following specific operations: adding lecithin and succinic acid monoglyceride to palm oil and stirring evenly to obtain pretreated palm oil; adding complex enzyme, glycerol, gelatin and chitosan to 8 kg of 0.15 mol / L acetic acid aqueous solution and stirring evenly, adding dropwise to the pretreated palm oil in a stirring state at a stirring speed of 1800 r / min, stirring for 15 minutes after the dropping is complete, adding ammonium sulfate solution with a mass fraction of 45% and stirring for 90 minutes, centrifuging and freeze-drying.
[0058] The activated bamboo fiber was prepared by the following specific operation: 8 kg of bamboo fiber was crushed and passed through a 60-mesh sieve, and was sent to 30 kg of 11 mol / L sodium hydroxide solution for soaking for 15 hours, filtered, washed with deionized water, dried, added to 30 kg of water, 1.5 kg of tetrabutyl titanate was added thereto, and ultrasonic treatment was performed for 20 minutes at an ultrasonic frequency of 12 kHz. The pH value of the system was adjusted to 8-9 with a 1 mol / L sodium hydroxide solution, and the ultrasonic treatment was continued for 90 minutes, centrifuged, washed with deionized water, and dried.
[0059] The preparation method of the above-mentioned degradable composite material includes the following steps: evenly mixing starch, poly-β-hydroxybutyrate, composite microspheres, and polyamide amine, adding activated bamboo fiber, crosslinking agent, and zinc stearate and continuing to stir for 15 minutes, putting into a mold, pressing at a low temperature of 55°C for 3 minutes, the pressing pressure is 2MPa, taking out after cooling, spraying a protective film, and ultraviolet sterilization.
[0060] Comparative Example 1
[0061] A degradable composite material, the raw materials of which include: 80kg starch, 15kg poly-β-hydroxybutyrate, 10kg composite microspheres, 2kg 5.0 generation polyamidoamine, 8kg activated bamboo fiber, 0.5kg crosslinking agent, and 1.5kg zinc stearate. The crosslinking agent is obtained by mixing sodium hexametaphosphate and sodium polyphosphate in a mass ratio of 1:0.5.
[0062] The raw materials of the composite microspheres include: 30kg palm oil, 2kg lecithin, 1.5kg succinic acid monoglyceride, 1.5kg composite enzyme, 1.5kg glycerol, 1.5kg gelatin, and 14kg ammonium sulfate. The composite enzyme includes: amylase with an enzyme activity of 15000U / g, cellulase with an enzyme activity of 3500U / g, and protease with an enzyme activity of 7500U / g.
[0063] The composite microspheres were prepared by the following specific operations: adding lecithin and succinic acid monoglyceride to palm oil and stirring evenly to obtain pretreated palm oil; adding complex enzyme, glycerol and gelatin to 8 kg of water and stirring evenly, and then dropping them into the pretreated palm oil in a stirring state at a stirring speed of 1800 r / min. After the dropping is complete, stirring for 15 minutes, adding ammonium sulfate solution with a mass fraction of 45% and stirring for 90 minutes, centrifuging and freeze-drying.
[0064] The activated bamboo fiber was prepared by the following specific operation: 8 kg of bamboo fiber was crushed and passed through a 60-mesh sieve, and was sent to 30 kg of 11 mol / L sodium hydroxide solution for soaking for 15 hours, filtered, washed with deionized water, dried, added to 30 kg of water, 1.5 kg of tetrabutyl titanate was added thereto, and ultrasonic treatment was performed for 20 minutes at an ultrasonic frequency of 12 kHz. The pH value of the system was adjusted to 8-9 with a 1 mol / L sodium hydroxide solution, and the ultrasonic treatment was continued for 90 minutes, centrifuged, washed with deionized water, and dried.
[0065] The preparation method of the above-mentioned degradable composite material includes the following steps: evenly mixing starch, poly-β-hydroxybutyrate, composite microspheres, and polyamide amine, adding activated bamboo fiber, crosslinking agent, and zinc stearate and continuing to stir for 15 minutes, putting into a mold, pressing at a low temperature of 55°C for 3 minutes, the pressing pressure is 2MPa, taking out after cooling, spraying a protective film, and ultraviolet sterilization.
[0066] Comparative Example 2
[0067] A degradable composite material, the raw materials of which include: 80kg starch, 15kg poly-β-hydroxybutyrate, 10kg composite microspheres, 8kg activated bamboo fiber, 0.5kg cross-linking agent, and 1.5kg zinc stearate. The cross-linking agent is obtained by mixing sodium hexametaphosphate and sodium polyphosphate in a mass ratio of 1:0.5.
[0068] The raw materials of the composite microspheres include: 30kg palm oil, 2kg lecithin, 1.5kg succinic acid monoglyceride, 1.5kg composite enzyme, 1.5kg glycerol, 1.5kg gelatin, 1.6kg chitosan, and 14kg ammonium sulfate. The composite enzyme includes: amylase with an enzyme activity of 15000U / g, cellulase with an enzyme activity of 3500U / g, and protease with an enzyme activity of 7500U / g.
[0069] The composite microspheres are prepared by the following specific operations: adding lecithin and succinic acid monoglyceride to palm oil and stirring evenly to obtain pretreated palm oil; adding complex enzyme, glycerol, gelatin and chitosan to 8 kg of 0.15 mol / L acetic acid aqueous solution and stirring evenly, adding dropwise to the pretreated palm oil in a stirring state at a stirring speed of 1800 r / min, stirring for 15 minutes after the dropping is complete, adding ammonium sulfate solution with a mass fraction of 45% and stirring for 90 minutes, centrifuging and freeze-drying.
[0070] The activated bamboo fiber was prepared by the following specific operation: 8 kg of bamboo fiber was crushed and passed through a 60-mesh sieve, and was sent to 30 kg of 11 mol / L sodium hydroxide solution for soaking for 15 hours, filtered, washed with deionized water, dried, added to 30 kg of water, 1.5 kg of tetrabutyl titanate was added thereto, and ultrasonic treatment was performed for 20 minutes at an ultrasonic frequency of 12 kHz. The pH value of the system was adjusted to 8-9 with a 1 mol / L sodium hydroxide solution, and the ultrasonic treatment was continued for 90 minutes, centrifuged, washed with deionized water, and dried.
[0071] The preparation method of the above-mentioned degradable composite material includes the following steps: mixing starch, poly-β-hydroxybutyrate, and composite microspheres evenly, adding activated bamboo fiber, crosslinking agent, and zinc stearate and continuing to stir for 15 minutes, putting into a mold, pressing at a low temperature of 55°C for 3 minutes, the pressing pressure is 2MPa, taking out after cooling, spraying a protective film, and ultraviolet sterilization.
[0072] The mechanical properties of the degradable composite materials obtained in Example 5 and Comparative Examples 1-2 were tested as follows:
[0073] Refer to GB / T 1040.2-2022 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics" for tensile strength and elongation at break;
[0074] Refer to GB / T 9341-2008 "Determination of flexural properties of plastics" for flexural strength determination;
[0075] Refer to GB / T 4857.5-92 "Drop test method for packaging and transport packages" to measure the drop height and record the maximum drop height of the sample without damage or cracks after falling.
[0076] like Figure 1 and Figure 2 As shown, the tensile strength and bending strength of the degradable composite material obtained in Example 5 are the largest, and the maximum drop height is also greater than that of Comparative Examples 1-2, which proves that the mechanical properties of the degradable composite material obtained in Example 5 are better than those of Comparative Examples 1-2 (P < 0.05).
[0077] The applicant believes that this is because the present invention adopts a compound of starch and poly-β-hydroxybutyrate, which has excellent biodegradability and thermoplastic processability, and combined with the activation of bamboo fiber, the product has excellent toughness; further adding polyamide amine containing a large number of active terminal amino groups, which can be more easily combined with the terminal carboxylic acid on the lecithin structure, and its special dendritic structure is entangled and compounded with the starch and poly-β-hydroxybutyrate molecular chain structure, so that the product has high static bending strength, no damage when falling, and excellent mechanical properties.
[0078] Referring to the preparation method of Example 5 and Comparative Examples 1-2, wherein the mold is a chopstick mold, the chopstick samples obtained in each group were subjected to water resistance (120h), acid resistance (6% acetic acid aqueous solution×120h) and hot oil resistance (180°C×10min), and it was found that no abnormalities visible to the naked eye (such as deformation, etc.) occurred in each group of samples, and the weight change was <±5%.
[0079] The degradation rate of the new groups of chopstick samples was tested using an automatic composting degradation tester. The experimental mixture was aerated at a controlled rate using air without carbon dioxide at 48±2°C, weak light, and steam conditions that do not affect the growth of microorganisms. The humidity was maintained at 80% RH. The degradation rate was determined by measuring the amount of carbon dioxide produced. The experiment lasted for 70 days. When the degradation rate exceeded 90%, the experiment of the group of samples was terminated.
[0080] like Figure 3 As shown, the degradation curves of the samples obtained in Example 5 and Comparative Example 2 are similar, and both are better than the sample obtained in Comparative Example 1.
[0081] The applicant believes that this is because both Example 5 and Comparative Example 2 use chitosan in combination with glycerol and gelatin. The chitosan molecule contains a large number of hydroxyl groups and amino groups, which can form stable hydrogen bonds with glycerol and gelatin to enhance the coating effect on the complex enzyme, and can also form microspheres through ammonium sulfate precipitation. Not only is the structure dense, but also the stability is excellent, and the contained complex enzyme can be effectively released during the degradation of chopsticks. The composite microspheres are compounded with starch and poly-β-hydroxybutyrate, and low-temperature processing is used, which can provide a good environment for the complex enzyme, effectively avoid direct contact between the complex enzyme and the material, reduce damage to the complex enzyme, and maintain high activity under high humidity, effectively adjust the degradation rate of the material, and thus achieve controllable degradation.
[0082] In comparative example 1, lecithin is combined with glycerol and gelatin to form a network structure of hydrogen bonds when the solvent evaporates, which significantly enhances the coating effect on the complex enzyme. However, the stability is poor and it is very easy to break in the subsequent process, resulting in direct contact between the complex enzyme and the material, reducing the survival rate and enzyme activity of the complex enzyme, thereby causing it to be unable to function normally during the degradation process, resulting in an unsatisfactory degradation curve for comparative example 1.
[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A degradable composite material, characterized in that: The raw materials include, by mass: 50-100 parts of starch, 10-20 parts of poly-β-hydroxybutyrate, 5-15 parts of composite microspheres, 1-3 parts of polyamidoamine, 5-10 parts of activated bamboo fiber, 0.1-1 parts of crosslinking agent, and 1-2 parts of plasticizer; The raw materials of the composite microspheres include, by weight: 20-40 parts of vegetable oil, 1-3 parts of lecithin, 1-2 parts of emulsifier, 1-2 parts of composite enzyme, 1-2 parts of glycerol, 1-2 parts of gelatin, 1-2 parts of chitosan, and 8-20 parts of ammonium sulfate; The activated bamboo fiber is obtained by depositing nano-titanium dioxide on the bamboo fiber after alkali washing.
2. The degradable composite material according to claim 1, characterized in that: The generation number of polyamidoamine is 4.0-6.
0.
3. The degradable composite material according to claim 1, characterized in that: Crosslinking agents include: Sodium hexametaphosphate and sodium polyphosphate; wherein the mass ratio of sodium hexametaphosphate to sodium polyphosphate is 1:0.1-1.
4. The degradable composite material according to claim 1, characterized in that: The plasticizer is calcium stearate and / or zinc stearate.
5. The degradable composite material according to claim 1, characterized in that: The vegetable oil is at least one of soybean oil, palm oil, corn oil, peanut oil and rapeseed oil; Preferably, the emulsifier is at least one of succinic acid monoglyceride, polyglycerol fatty acid ester, and sucrose fatty acid ester.
6. The degradable composite material according to claim 1, characterized in that: The complex enzyme comprises amylase, cellulase and protease; the enzymatic activity of amylase is 10000-20000U / g, the enzymatic activity of cellulase is 3000-4000U / g, and the enzymatic activity of protease is 6000-9000U / g.
7. The degradable composite material according to claim 1, characterized in that: The composite microspheres are prepared by the following specific operations: adding lecithin and an emulsifier to vegetable oil and stirring evenly to obtain pretreated vegetable oil; adding complex enzyme, glycerol, gelatin and chitosan to an acetic acid aqueous solution and stirring evenly, adding dropwise to the pretreated vegetable oil in a stirring state, stirring for 10-20 minutes after the dropping is complete, adding an ammonium sulfate solution and stirring for 1-2 hours, centrifuging and freeze-drying.
8. The degradable composite material according to claim 1, characterized in that: The activated bamboo fiber is prepared by the following specific operations: the bamboo fiber is crushed and sieved, sent into a sodium hydroxide solution to soak for 10-20 hours, filtered, washed, dried, added to water, tetrabutyl titanate is added thereto and ultrasonically treated for 10-30 minutes, the pH value of the system is adjusted to 8-9, the ultrasonic treatment is continued for 1-2 hours, centrifuged, washed, and dried.
9. A method for preparing the degradable composite material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: uniformly mixing starch, poly-β-hydroxybutyrate, composite microspheres and polyamide amine, adding activated bamboo fiber, crosslinking agent and plasticizer and continuing stirring for 10-20 minutes, placing into a mold, and pressing at a low temperature of 50-60° C. for 1-5 minutes with a pressing pressure of 1-3 MPa.
10. Use of the degradable composite material according to any one of claims 1 to 8 in chopsticks.