Starch-based degradable plastic and preparation method thereof
By using specific dispersants, plasticizers, crosslinkers and nanoparticles in starch-based degradable plastics and undergoing plastic modification, the starch-based degradable plastics has strong hydrophilicity, brittle texture and thermal stability. The problem of poor performance has achieved improvements in the strength, heat resistance and water resistance of the material.
Patent Information
- Application Number
- CN202411339113.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-12
AI Technical Summary
Existing starch-based degradable plastics have problems such as strong hydrophilicity, brittle texture and poor thermal stability.
Use titanate, stearic acid, oleic acid or sodium polyacrylate as dispersants, phthalate, aliphatic dibasic acid, fatty acid esters, benzene polyacrylate, polyol esters or alkyl sulfonic acid Esters as plasticizers, epoxychlorohydrin, N,N'methylenebisacrylamide, diethylenetriamine, triethylenetetramine, divinylbenzene as crosslinking agents, and by polylactic acid and Polyvinyl alcohol is blended, modified silica nanoparticles are added, and plasticized and modified with glycerol and sorbitol to form a starch-based degradable plastic.
It improves the waterproofing, mechanical and processing properties of starch-based degradable plastics, enhances the strength and thermal stability of the material, reduces water absorption, and improves the heat and water resistance of the material.
Smart Images

Figure BDA0005059167300000021 
Figure FDA0005059167290000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a starch-based degradable plastic and a preparation method thereof. Background Art
[0002] Plastics are not only widely used in our daily lives, but have also become one of the four pillars of the material field due to their low density, high strength, good chemical stability, and low price. However, the extensive use of plastics has produced a lot of disposable plastic waste that cannot be recycled, causing increasingly serious "white pollution", such as groundwater and soil pollution, and the destruction of animal and plant resources, which seriously endangers human survival and health.
[0003] Starch has the characteristics of being renewable, cheap, easy to store and transport. Under certain conditions, it can undergo various reactions and derive many derivatives. The good recyclability and biodegradability of starch make it an excellent raw material for biodegradable materials. Among them, starch-based degradable plastics are widely used, and the demand is increasing year by year. Starch-based degradable plastics are divided into starch-filled plastics, starch-blended plastics, and all-starch plastics. However, the starch-based degradable plastics in the existing schemes mainly have the following defects: although the excessive starch content improves the degradability of the material, it will reduce the tensile strength and elongation at break of the material; due to the presence of a large number of hydroxyl groups on the starch surface, the material has a certain water absorption and a high water absorption rate; the high starch content leads to low heat resistance and poor thermal stability of the material. Therefore, how to increase the strength and thermal stability of the material and reduce its water absorption rate while ensuring that the starch-based plastic has a high degradation rate is a problem that needs to be solved urgently. Summary of the invention
[0004] The purpose of the present invention is to provide a starch-based biodegradable plastic and a preparation method thereof, to solve the following technical problems:
[0005] Existing starch-based biodegradable plastics have the problems of strong hydrophilicity, brittle texture and poor thermal stability.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A starch-based degradable plastic, characterized in that the starch-based degradable plastic comprises at least the following components:
[0008]
[0009] As a further solution of the present invention: the dispersant is at least one of titanate, stearic acid, oleic acid or sodium polyacrylate.
[0010] As a further embodiment of the present invention: the plasticizer is at least one of phthalic acid esters, aliphatic dibasic acid esters, fatty acid esters, benzene polyesters, polyol esters, epoxy hydrocarbons or alkyl sulfonates.
[0011] As a further embodiment of the present invention: the cross-linking agent is at least one of epichlorohydrin, N,N'-methylenebisacrylamide, diethylenetriamine, triethylenetetramine and divinylbenzene.
[0012] A method for preparing a starch-based degradable plastic as claimed in any one of claims 1 to 5, characterized in that it comprises at least the following steps:
[0013] The starch is placed in a vacuum drying oven to dry, a plasticizing modifier is added, the mixture is mechanically stirred by a high-speed stirrer, and after being fully mixed, it is sealed with a PE packaging bag, and the mixture is further dried in a vacuum drying oven, and melt blended by a Harp torque rheometer to obtain plasticized starch;
[0014] The nano-silicon dioxide powder is dispersed in ethanol, a coupling agent is added, and after the reaction is modified by stirring, polyethylene glycol is added, and ultrasonic dispersion is performed. After the reaction is completed, the modified silicon dioxide nanoparticles are obtained by filtering, washing, and drying.
[0015] Preparation of starch-based biodegradable plastics: Plasticized starch, polylactic acid and polyvinyl alcohol are weighed according to a weight ratio and added to a grinder for grinding to obtain a powder mixture, and then plasticizers, cross-linking agents, dispersants and modified silica nanoparticles are added for continued blending to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation, and blow molding to form a starch-based biodegradable plastic.
[0016] As a further embodiment of the present invention: the starch is at least one of corn starch, tapioca starch, rice starch or wheat starch.
[0017] As a further embodiment of the present invention: the plasticizing modifier comprises at least glycerol and sorbitol.
[0018] As a further solution of the present invention: the solid-liquid ratio of the nano-silicon dioxide powder to the ethanol is 1:50-100, the coupling agent is at least one of a silane coupling agent, a titanate coupling agent or an aluminate coupling agent, and the ultrasonic dispersion time is 20-30 minutes.
[0019] Beneficial effects of the present invention:
[0020] (1) The present invention uses starch as a matrix and mixes it with polylactic acid and polyvinyl alcohol to prepare starch-based degradable plastics. The prepared starch-based degradable plastics have good waterproof properties, mechanical properties and processing properties, can well replace petroleum-based plastics, and have good application prospects. Starch macromolecules and polyvinyl alcohol have a strong degree of hydroxyl bonding, and the molecules can be tightly combined, which improves the stability of the system and increases the strength of the plastic products finally prepared; polylactic acid is introduced into the blending system. On the one hand, polyvinyl alcohol can enhance the crystallinity of polylactic acid in the blending system and adjust the mechanical properties of the prepared starch-based degradable plastics. On the other hand, it can reduce the use of polyvinyl alcohol, thereby improving the thermal stability and water resistance of the starch-based degradable plastics. The present invention also performs plasticization modification on starch, which can solve the problem of poor compatibility between starch and polylactic acid and polyvinyl alcohol, reduce small molecule plasticizers such as glycerol, improve the strength and toughness of the composite material, and reduce the overall cost of the product.
[0021] (2) The present invention adds modified silicon dioxide nanoparticles to the starch, polylactic acid and polyvinyl alcohol blending system. Silicon dioxide is an inorganic rigid particle that can withstand a large external force, so it can give the starch-based degradable plastic prepared by the present invention excellent tensile strength, making the plastic have a certain elasticity, and the modified silicon dioxide nanoparticles have greatly improved dispersibility, which can reduce the interface effect with polyvinyl alcohol and polylactic acid, and further strengthen the mechanical properties of the blended material. At the same time, adding modified silicon dioxide nanoparticles can also improve the heat resistance and water resistance of the starch-based degradable plastic.
[0022] (3) The present invention uses glycerol and sorbitol to plasticize and modify starch. Both glycerol and sorbitol destroy the hydrogen bonds in the starch structure through the hydroxyl groups in their structures, reduce the polarity between starch molecules, and achieve the purpose of plasticization. Due to its small molecular volume, glycerol is easier to enter the starch molecule, combine with the hydroxyl groups on the starch molecule, form new hydrogen bonds, support the starch molecules with the original spiral structure, destroy the crystalline structure, and make the starch molecules loose, so that it becomes a thermoplastic starch with certain mechanical properties. In addition, during the processing of starch, the glycerol molecules are small and have a certain lubricating effect. The hydrogen bonds are easily destroyed and the processing performance is good. On the other hand, sorbitol can form strong hydrogen bonds with starch, but the molecules are large and the movement in the starch molecules is restricted. Only a small part can enter the starch molecules. In addition to being a plasticizer, sorbitol can also act as a physical cross-linking agent in the starch molecule, linking starch to starch, and having a certain effect on the enhancement of starch. By adjusting the ratio of glycerol to sorbitol, the prepared starch-based degradable plastic has good processing performance and mechanical properties. DETAILED DESCRIPTION
[0023] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1
[0025] The preparation method of modified silicon dioxide nanoparticles comprises the following steps:
[0026] 3 parts by mass of nano-silica powder were dried at 105°C for 24 hours, dispersed in ethanol at a ratio of 1:100, 0.05 parts by mass of titanate coupling agent were added, and after stirring and reacting at 60°C for 80 minutes, 0.1 parts by mass of polyethylene glycol were added, and ultrasonic dispersion was performed for 30 minutes to obtain modified silica nanoparticles;
[0027] The preparation method of plasticized starch comprises the following steps:
[0028] First, 60 parts by mass of starch were placed in a vacuum drying oven at 80°C for 5 hours, and then 2 parts by mass of glycerol and 1 part by mass of sorbitol were added to the starch, and after being fully mixed by mechanical stirring with a high-speed stirrer, the mixture was sealed with a PE packaging bag and placed in a vacuum drying oven at 80°C for 12 hours. The mixture was melt blended by a Harp torque rheometer at a mixing temperature of 120°C and a rotation speed of 40 r / min to obtain plasticized starch.
[0029] The preparation method of starch-based biodegradable plastic comprises the following steps:
[0030] 60 parts by weight of plasticized starch, 30 parts by weight of polylactic acid and 30 parts by weight of polyvinyl alcohol are weighed according to a weight ratio and added into a pulverizer for pulverization to obtain a powder mixture, 1 part by weight of a plasticizer, 2 parts by weight of a dispersant and 3 parts by weight of modified silicon dioxide nanoparticles are added and the mixture is continuously blended for 5-10 minutes, and then 5 parts by weight of a cross-linking agent is added and mixed for 3-5 minutes to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation and blow molding to form a starch-based biodegradable plastic.
[0031] Example 2
[0032] The preparation method of modified silicon dioxide nanoparticles comprises the following steps:
[0033] 3 parts by mass of nano-silica powder were dried at 105°C for 24 hours, dispersed in ethanol at a ratio of 1:100, 0.05 parts by mass of titanate coupling agent were added, and after stirring and reacting at 60°C for 80 minutes, 0.1 parts by mass of polyethylene glycol were added, and ultrasonic dispersion was performed for 30 minutes to obtain modified silica nanoparticles;
[0034] The preparation method of plasticized starch comprises the following steps:
[0035] First, 60 parts by mass of starch were placed in a vacuum drying oven at 80°C for 5 hours, and then 2 parts by mass of glycerol and 1 part by mass of sorbitol were added to the starch, and after being fully mixed by mechanical stirring with a high-speed stirrer, the mixture was sealed with a PE packaging bag and placed in a vacuum drying oven at 80°C for 12 hours. The mixture was melt blended by a Harp torque rheometer at a mixing temperature of 120°C and a rotation speed of 40 r / min to obtain plasticized starch.
[0036] The preparation method of starch-based biodegradable plastic comprises the following steps:
[0037] 60 parts by weight of plasticized starch, 30 parts by weight of polylactic acid and 30 parts by weight of polyvinyl alcohol are weighed according to a weight ratio and added into a pulverizer for pulverization to obtain a powder mixture, 1 part by weight of a plasticizer, 2 parts by weight of a dispersant and 2 parts by weight of modified silicon dioxide nanoparticles are added and blended for 5-10 minutes, and then 5 parts by weight of a cross-linking agent are added and mixed for 3-5 minutes to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation, and blow molding to form a starch-based biodegradable plastic.
[0038] Example 3
[0039] The preparation method of modified silicon dioxide nanoparticles comprises the following steps:
[0040] 3 parts by mass of nano-silica powder were dried at 105°C for 24 hours, dispersed in ethanol at a ratio of 1:100, 0.05 parts by mass of titanate coupling agent were added, and after stirring and reacting at 60°C for 80 minutes, 0.1 parts by mass of polyethylene glycol were added, and ultrasonic dispersion was performed for 30 minutes to obtain modified silica nanoparticles;
[0041] The preparation method of plasticized starch comprises the following steps:
[0042] First, 60 parts by mass of starch were placed in a vacuum drying oven at 80°C for 5 hours, and then 2 parts by mass of glycerol and 1 part by mass of sorbitol were added to the starch, and after being fully mixed by mechanical stirring with a high-speed stirrer, the mixture was sealed with a PE packaging bag and placed in a vacuum drying oven at 80°C for 12 hours. The mixture was melt blended by a Harp torque rheometer at a mixing temperature of 120°C and a rotation speed of 40 r / min to obtain plasticized starch.
[0043] The preparation method of starch-based biodegradable plastic comprises the following steps:
[0044] 60 parts by weight of plasticized starch, 30 parts by weight of polylactic acid and 30 parts by weight of polyvinyl alcohol are weighed according to a weight ratio and added into a pulverizer for pulverization to obtain a powder mixture, 1 part by weight of a plasticizer, 2 parts by weight of a dispersant and 1 part by weight of modified silicon dioxide nanoparticles are added and blended for 5-10 minutes, and then 5 parts by weight of a cross-linking agent are added and mixed for 3-5 minutes to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation, and blow molding to form a starch-based biodegradable plastic.
[0045] Example 4
[0046] The preparation method of modified silicon dioxide nanoparticles comprises the following steps:
[0047] 3 parts by mass of nano-silica powder were dried at 105°C for 24 hours, dispersed in ethanol at a ratio of 1:100, 0.05 parts by mass of titanate coupling agent were added, and after stirring and reacting at 60°C for 80 minutes, 0.1 parts by mass of polyethylene glycol were added, and ultrasonic dispersion was performed for 30 minutes to obtain modified silica nanoparticles;
[0048] The preparation method of plasticized starch comprises the following steps:
[0049] First, 60 parts by mass of starch were placed in a vacuum drying oven at 80°C and dried for 5 hours, then 1 part by mass of glycerol and 2 parts by mass of sorbitol were added to the starch, and after being fully mixed by mechanical stirring with a high-speed stirrer, the mixture was sealed with a PE packaging bag and placed in a vacuum drying oven at 80°C for 12 hours. Melt blending was performed using a Harp torque rheometer, with a mixing temperature of 120°C and a rotation speed of 40 r / min to obtain plasticized starch;
[0050] The preparation method of starch-based biodegradable plastic comprises the following steps:
[0051] 60 parts by weight of plasticized starch, 30 parts by weight of polylactic acid and 30 parts by weight of polyvinyl alcohol are weighed according to a weight ratio and added into a pulverizer for pulverization to obtain a powder mixture, 1 part by weight of a plasticizer, 2 parts by weight of a dispersant and 3 parts by weight of modified silicon dioxide nanoparticles are added and the mixture is continuously blended for 5-10 minutes, and then 5 parts by weight of a cross-linking agent is added and mixed for 3-5 minutes to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation and blow molding to form a starch-based biodegradable plastic.
[0052] Example 5
[0053] The preparation method of modified silicon dioxide nanoparticles comprises the following steps:
[0054] 3 parts by mass of nano-silica powder were dried at 105°C for 24 hours, dispersed in ethanol at a ratio of 1:100, 0.05 parts by mass of titanate coupling agent were added, and after stirring and reacting at 60°C for 80 minutes, 0.1 parts by mass of polyethylene glycol were added, and ultrasonic dispersion was performed for 30 minutes to obtain modified silica nanoparticles;
[0055] The preparation method of plasticized starch comprises the following steps:
[0056] First, 60 parts by mass of starch were placed in a vacuum drying oven at 80°C for 5 hours, and then 1.5 parts by mass of glycerol and 1.5 parts by mass of sorbitol were added to the starch, and the mixture was fully mixed by mechanical stirring with a high-speed stirrer, and then sealed with a PE packaging bag and placed in a vacuum drying oven at 80°C for 12 hours. The mixture was melt blended by a Harp torque rheometer at a mixing temperature of 120°C and a rotation speed of 40 r / min to obtain plasticized starch.
[0057] The preparation method of starch-based biodegradable plastic comprises the following steps:
[0058] 60 parts by weight of plasticized starch, 30 parts by weight of polylactic acid and 30 parts by weight of polyvinyl alcohol are weighed according to a weight ratio and added into a pulverizer for pulverization to obtain a powder mixture, 1 part by weight of a plasticizer, 2 parts by weight of a dispersant and 3 parts by weight of modified silicon dioxide nanoparticles are added and the mixture is continuously blended for 5-10 minutes, and then 5 parts by weight of a cross-linking agent is added and mixed for 3-5 minutes to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation and blow molding to form a starch-based biodegradable plastic.
[0059] Example 6
[0060] The preparation method of modified silicon dioxide nanoparticles comprises the following steps:
[0061] 3 parts by mass of nano-silica powder were dried at 105°C for 24 hours, dispersed in ethanol at a ratio of 1:100, 0.05 parts by mass of titanate coupling agent were added, and after stirring and reacting at 60°C for 80 minutes, 0.1 parts by mass of polyethylene glycol were added, and ultrasonic dispersion was performed for 30 minutes to obtain modified silica nanoparticles;
[0062] The preparation method of plasticized starch comprises the following steps:
[0063] First, 60 parts by mass of starch were placed in a vacuum drying oven at 80°C for 5 hours, and then 2 parts by mass of glycerol and 1 part by mass of sorbitol were added to the starch, and after being fully mixed by mechanical stirring with a high-speed stirrer, the mixture was sealed with a PE packaging bag and placed in a vacuum drying oven at 80°C for 12 hours. The mixture was melt blended by a Harp torque rheometer at a mixing temperature of 120°C and a rotation speed of 40 r / min to obtain plasticized starch.
[0064] The preparation method of starch-based biodegradable plastic comprises the following steps:
[0065] 60 parts by weight of plasticized starch, 40 parts by weight of polylactic acid and 30 parts by weight of polyvinyl alcohol are weighed according to a weight ratio and added into a pulverizer for pulverization to obtain a powder mixture, 1 part by weight of a plasticizer, 2 parts by weight of a dispersant and 3 parts by weight of modified silicon dioxide nanoparticles are added and blended for 5-10 minutes, and then 5 parts by weight of a cross-linking agent are added and mixed for 3-5 minutes to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation, and blow molding to form a starch-based biodegradable plastic.
[0066] Comparative Example 1
[0067] Compared with Example 1, the preparation of modified silica nanoparticles is omitted in Comparative Example 1, and silica particles are not added in the preparation of starch-based degradable plastics. The remaining components and preparation methods are completely consistent with those in Example 1.
[0068] Comparative Example 2
[0069] Compared with Example 1, Comparative Example 2 omits the preparation of modified silica nanoparticles, and directly adds 3 parts by mass of unmodified silica nanoparticles in the preparation step of starch-based degradable plastic. The remaining components and preparation method are completely consistent with Example 1.
[0070] Comparative Example 3
[0071] Compared with Example 1, Comparative Example 3 omits the preparation of plasticized starch, and directly adds 60 parts by mass of unmodified starch in the preparation of starch-based biodegradable plastic, increases the content of plasticizer to 3 parts by mass, and the remaining components and preparation method are exactly the same as those in Example 1.
[0072] Comparative Example 4
[0073] Compared with Example 1, in the step of preparing plasticized starch, 3 parts by mass of glycerol was added to plasticize and modify the starch in Comparative Example 4, and sorbitol was not introduced. The remaining components and preparation method were completely consistent with those in Example 1.
[0074] Comparative Example 5
[0075] Compared with Example 1, in Comparative Example 5, polylactic acid is not added for blending in the preparation of starch-based biodegradable plastic, and the remaining components and preparation method are completely consistent with those of Example 1.
[0076] Comparative Example 6
[0077] Compared with Example 1, in Comparative Example 6, 60 parts by mass of polylactic acid are blended in the preparation of the starch-based degradable plastic, and the remaining components and the preparation method are completely consistent with those of Example 1.
[0078] Performance Testing
[0079] Mechanical properties
[0080] The starch-based degradable plastic samples in Examples 1-6 and Comparative Examples 1-6 were injection molded into tensile test strips by an injection molding machine, and the tensile strength and elongation at break of the test strips were measured according to the third part of GB / T1040.3-2006 "Determination of tensile properties of plastics". The test results are shown in Table 1;
[0081] Table 1 Test results of tensile strength and elongation at break of Examples 1-6 and Comparative Examples 1-6
[0082] Tensile strength / MPa Elongation at break / % Example 1 30.2 7.4 Example 2 28.8 6.9 Example 3 27.6 7.1 Example 4 28.6 6.4 Example 5 26.9 6.8 Example 6 29.1 6.8 Comparative Example 1 16.3 4.3 Comparative Example 2 14.2 5.2 Comparative Example 3 17.9 4.8 Comparative Example 4 21.2 4.6 Comparative Example 5 9.2 2.8 Comparative Example 6 20.1 1.2
[0083] As shown in Table 1, the data of Examples 1-6 show that the tensile strength and elongation at break of the starch-based degradable plastic prepared by the present invention are improved. Comparing Examples 1-3 with Comparative Examples 1 and 2, adding a certain amount of modified silicon dioxide nanoparticles increases the tensile strength and fracture growth rate of the obtained plastic samples, and the modified silicon dioxide nanoparticles have a more excellent improvement effect, indicating that adding a small amount of modified silicon dioxide nanoparticles can improve the toughness of starch, polylactic acid, and polyvinyl alcohol blends. Comparing Examples 1, 4, 5 with Comparative Examples 3 and 4, after the starch is plasticized and modified, the mechanical properties of the plastic samples are effectively improved. The modification effect of the mixture of glycerol and sorbitol is better than that of the single use of glycerol, and the use of plasticizers can be reduced. Comparing Examples 1 and 6 with Comparative Examples 5 and 6, the content of polylactic acid also has a great influence on the mechanical properties of the blend of starch, polyvinyl alcohol and polylactic acid. Adding a certain amount of polylactic acid has a certain effect on the elongation at break of the material, and adding excessive polylactic acid will make the blend brittle.
[0084] Water vapor transmission rate
[0085] The starch-based degradable plastic samples in Examples 1-6 and Comparative Examples 1-6 were injection molded into tensile test strips by an injection molding machine. The test strips were tested using a TGA thermogravimetric analysis system in a nitrogen atmosphere. The N2 flow rate was 100 mL / min, and the temperature was increased from 30°C to 600°C at a heating rate of 10°C / min. The temperature at which the thermal weight loss was 5% was tested and recorded as the starting thermal decomposition temperature. The water absorption rate was tested according to GB / T1034-2008 standard. The 24h water absorption rate of the test strips was measured using W3 / 030. The test results are shown in Table 2.
[0086] Table 2 Water vapor transmission rate test results of Examples 1-6 and Comparative Examples 1-6
[0087] Initial thermal decomposition temperature / ℃ Total water absorption after 24h immersion / % Example 1 289 0.15 Example 2 278 0.24 Example 3 265 0.34 Example 4 246 0.25 Example 5 284 0.36 Example 6 276 0.26 Comparative Example 1 177 0.27 Comparative Example 2 220 0.24 Comparative Example 3 213 1.56 Comparative Example 4 224 1.34 Comparative Example 5 201 2.86 Comparative Example 6 232 1.49
[0088] As can be seen from Table 2, the data of Examples 1-6 show that the starch-based degradable plastic prepared by the present invention makes the material have good heat resistance and water resistance. Comparing Examples 1-3 with Comparative Examples 1 and 2, adding a certain amount of modified silicon dioxide nanoparticles can effectively improve the heat resistance and water resistance of starch-based degradable plastic samples. Comparing Examples 1, 4, 5 with Comparative Examples 3 and 4, after the starch is plasticized and modified, the use of plasticizers such as glycerol is reduced, and the water resistance of the plastic samples is effectively improved. Comparing Examples 1 and 6 with Comparative Examples 5 and 6, the addition of polylactic acid can improve the effect of polyvinyl alcohol on the heat resistance and water resistance of starch-based plastics.
[0089] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A starch-based biodegradable plastic, characterized in that: The starch-based degradable plastic comprises at least the following components:
2. A starch-based biodegradable plastic according to claim 1, characterized in that: The dispersant is at least one of titanate, stearic acid, oleic acid or sodium polyacrylate.
3. A starch-based biodegradable plastic according to claim 1, characterized in that: The plasticizer is at least one of phthalate, aliphatic dibasic acid ester, fatty acid ester, benzene polyester, polyol ester, epoxy hydrocarbon or alkyl sulfonate.
4. The starch-based degradable plastic according to claim 1, characterized in that: The cross-linking agent is at least one of epichlorohydrin, N,N'methylenebisacrylamide, diethylenetriamine, triethylenetetramine and divinylbenzene.
5. A method for preparing the starch-based degradable plastic according to any one of claims 1 to 4, characterized in that: At least the following steps are included: The starch is placed in a vacuum drying oven to dry, a plasticizing modifier is added, the mixture is mechanically stirred by a high-speed stirrer, and after being fully mixed, it is sealed with a PE packaging bag, and the mixture is further dried in a vacuum drying oven, and melt blended by a Harp torque rheometer to obtain plasticized starch; The nano-silicon dioxide powder is dispersed in ethanol, a coupling agent is added, and after the reaction is modified by stirring, polyethylene glycol is added, and ultrasonic dispersion is performed. After the reaction is completed, the modified silicon dioxide nanoparticles are obtained by filtering, washing, and drying. Preparation of starch-based biodegradable plastics: Plasticized starch, polylactic acid and polyvinyl alcohol are weighed according to a weight ratio and added to a grinder for grinding to obtain a powder mixture, and then plasticizers, cross-linking agents, dispersants and modified silica nanoparticles are added for continued blending to form a mixed raw material, and the mixed raw material is put into a twin-screw granulator for extrusion, granulation, and blow molding to form a starch-based biodegradable plastic.
6. The method for preparing a starch-based degradable plastic according to claim 5, characterized in that: The starch is at least one of corn starch, tapioca starch, rice starch or wheat starch.
7. The method for preparing a starch-based degradable plastic according to claim 5, characterized in that: The plasticizing modifier includes at least glycerol and sorbitol.
8. The method for preparing a starch-based degradable plastic according to claim 5, characterized in that: The solid-liquid ratio of the nano-silicon dioxide powder to the ethanol is 1:50-100, the coupling agent is at least one of a silane coupling agent, a titanate coupling agent or an aluminate coupling agent, and the ultrasonic dispersion time is 20-30 minutes.