Flame-retardant polyolefin material and preparation method thereof

By preparing a flame-retardant polyolefin material containing high-density polyethylene, ethylene-vinyl acetate copolymer, modified magnesium hydroxide, etc., the problem of traditional PVC materials producing toxic gases and thick smoke during fire is solved, and the problem of traditional PVC materials is realized. Low smoke, non-toxic, environmentally friendly flame retardant effect and good flame retardant performance.

CN118931013AInactive Publication Date: 2024-11-12FOSHAN NAIYI SOLUBLE NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411182519.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional PVC materials produce a large amount of toxic gases and highly toxic smoke during fires, resulting in more than 80% of the causes of death in fire accidents are related to the thick smoke and toxic gases produced by the materials, and it is difficult to prevent the flame from spreading, affecting safe evacuation and rescue.

Method used

A flame retardant polyolefin material is used, and the composition includes high-density polyethylene, ethylene-vinyl acetate copolymer, modified magnesium hydroxide, flame retardant, processing aid and antioxidant, and is mixed by intensive refining and plasticizing. The step extrusion and die surface hot granulation process are prepared to form a low-smoke, non-toxic and environmentally friendly flame retardant material.

Benefits of technology

It improves the flame retardant and mechanical properties of the material, reduces the amount of smoke, ensures safety and environmental protection in fire situations, and provides good flame retardant effect and low toxicity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012606450000131
    Figure BDA0005012606450000131
  • Figure BDA0005012606450000141
    Figure BDA0005012606450000141
Patent Text Reader

Abstract

The invention provides a flame-retardant polyolefin material and a preparation method thereof, and belongs to the related technical field of flame-retardant materials. The flame-retardant polyolefin material comprises the following components in parts by weight: 70-75 parts of a high-density polyethylene material, 25-30 parts of an ethylene-vinyl acetate copolymer, 65-75 parts of modified magnesium hydroxide, 7-9 parts of a flame retardant, 5-7 parts of a processing aid and 2-3 parts of an antioxidant. The flame-retardant polyolefin material prepared by the preparation method disclosed by the invention is good in tensile property and flame-retardant property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field related to flame retardant materials, and in particular to a flame retardant polyolefin material and a preparation method thereof. Background Art

[0002] In recent years, people have found that more than 80% of the causes of death in fire accidents are related to the thick smoke and toxic gases produced by materials. With the rapid development of my country's modern industry, safety prevention measures have become more and more perfect. In many large public places, in order to avoid secondary disasters caused by building fires (a large amount of smoke and acidic gases are produced during combustion), building materials are required to have flame retardant properties such as preventing the spread of flames, and building materials are required to have low smoke and low gas corrosiveness during combustion, which is conducive to the safe evacuation of workers from the scene. That is, building materials are required to have halogen-free, low smoke, flame retardant and other properties when burning.

[0003] Traditional PVC (polyvinyl chloride) easily decomposes when heated during a fire, emitting a large amount of highly toxic and corrosive HCL (hydrogen chloride) gas and a large amount of highly toxic smoke, which can easily cause significant loss of life and property, and bring great difficulties to rescue work. Summary of the invention

[0004] 1. Technical issues to be solved

[0005] In view of the deficiencies in the prior art, the present invention provides a flame retardant polyolefin material and a preparation method thereof.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A flame retardant polyolefin material comprises the following components: by weight, 70-75 parts of high-density polyethylene material, 25-30 parts of ethylene-vinyl acetate copolymer, 65-75 parts of modified magnesium hydroxide, 7-9 parts of flame retardant, 5-7 parts of processing aid and 2-3 parts of antioxidant.

[0009] Furthermore, the high-density polyethylene material is HDPE, and the mass fraction of acetic acid in the ethylene-vinyl acetate copolymer is 26-30%.

[0010] Furthermore, the preparation method of the modified magnesium hydroxide is as follows: according to parts by weight, 3 to 3.5 parts of silane coupling agent and 2 to 2.5 parts of titanate are dissolved in 44 to 50 parts of anhydrous ethanol to form a mixed solution, and then 98 to 102 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added to the mixed solution, and dried at 80 to 85 degrees for 10 to 12 hours to obtain modified magnesium hydroxide.

[0011] Furthermore, the silane coupling agent is one of KH550 and KH560 or a mixture of the two in any proportion.

[0012] Furthermore, the flame retardant is red phosphorus.

[0013] Furthermore, the processing aid includes 1 part of polyethylene wax and 3 to 4 parts of white oil by weight.

[0014] Furthermore, the antioxidant is BASF Irganox133.

[0015] A method for preparing a flame retardant polyolefin material comprises the following steps:

[0016] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 130-160°C to obtain a rubber mixture after mixing evenly;

[0017] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0018] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0019] S4: The finished rubber particles can be packaged, tested and put into storage.

[0020] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0021] 1. The surface of magnesium hydroxide contains many hydroxyl (-OH) groups. Hydroxyl is a hydrophilic group, and hydroxyl can also undergo condensation reactions with many substances.

[0022] 2. The alkoxy group in the silane coupling agent is a polar group that can react with the -OH of Mg(OH)2. The other part of the group, the alkyl group, can diffuse into the interface area of ​​the polyolefin and react with the macromolecular chain, making the nano-Mg(OH)2 more closely combined with the matrix HDPE, more evenly dispersed, and with better mechanical properties, while also improving the flame retardant effect of the flame-retardant polyolefin material. In addition, a small amount of silane can use the trace moisture on the surface of the particles (such as crystal water, bound water) to generate silanol [-Si(OH)3]; it can also form hydrogen bonds with the -OH on the surface of Mg(OH)2 to enhance the connection between the two.

[0023] 3. HDPE has excellent mechanical properties and low smoke emission. EVA molecules have polar bonds and are compatible with inorganic fillers. Blending EVA and EIDPE can produce a skeleton material with excellent mechanical properties and good compatibility with inorganic fillers.

[0024] 4. The flame-retardant polyolefin material prepared by the present invention is low-smoke, non-toxic, environmentally friendly, and has good flame retardancy. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] BASF Irganox 133 was purchased from Shanghai Anhui Chemical Co., Ltd.

[0027] KH550 and KH560 were purchased from Shandong Bosheng Chemical Co., Ltd.

[0028] Example 1

[0029] A flame retardant polyolefin material comprises the following components: by weight, 75 parts of high-density polyethylene material, 25 parts of ethylene-vinyl acetate copolymer, 70 parts of modified magnesium hydroxide, 8 parts of flame retardant, 6 parts of processing aid and 2.5 parts of antioxidant.

[0030] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 28%.

[0031] Preparation method of modified magnesium hydroxide: According to parts by weight, 3.5 parts of silane coupling agent and 2.5 parts of titanate are dissolved in 44 parts of anhydrous ethanol to form a mixed solution, and then 100 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added to the mixed solution, and dried at 80° C. for 10 hours to obtain modified magnesium hydroxide.

[0032] The silane coupling agent is KH550.

[0033] The flame retardant is red phosphorus.

[0034] The processing aid is prepared by mixing 1 part of polyethylene wax and 3.5 parts of white oil by weight.

[0035] The antioxidant was BASF Irganox133.

[0036] A method for preparing a flame retardant polyolefin material is as follows:

[0037] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 145°C to obtain a rubber mixture after mixing evenly;

[0038] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0039] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0040] S4: The finished rubber particles can be packaged, tested and put into storage.

[0041] Example 2

[0042] A flame retardant polyolefin material comprises the following components: by weight, 70 parts of high-density polyethylene material, 25 parts of ethylene-vinyl acetate copolymer, 65 parts of modified magnesium hydroxide, 7 parts of flame retardant, 5 parts of processing aid and 2 parts of antioxidant.

[0043] High density polyethylene material is HDPE.

[0044] The mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 26%.

[0045] Preparation method of modified magnesium hydroxide: According to parts by weight, 3 parts of silane coupling agent and 2 parts of titanate are dissolved in 44 parts of anhydrous ethanol to form a mixed solution, and then 98 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added to the mixed solution, and dried at 80° C. for 10 hours to obtain modified magnesium hydroxide.

[0046] The silane coupling agent is a mixture of KH550 and KH560, wherein the mass ratio of KH550 to KH560 is 1:1.

[0047] The flame retardant is red phosphorus.

[0048] The processing aid is prepared by mixing 1 part of polyethylene wax and 3 parts of white oil by weight.

[0049] The antioxidant was BASF Irganox133.

[0050] A method for preparing a flame retardant polyolefin material comprises the following steps:

[0051] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 130°C to obtain a rubber mixture after mixing evenly;

[0052] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0053] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0054] S4: The finished rubber particles can be packaged, tested and put into storage.

[0055] Example 3

[0056] A flame retardant polyolefin material comprises the following components: by weight, 75 parts of high-density polyethylene material, 30 parts of ethylene-vinyl acetate copolymer, 75 parts of modified magnesium hydroxide, 9 parts of flame retardant, 7 parts of processing aid and 3 parts of antioxidant.

[0057] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in the ethylene-vinyl acetate copolymer is 30%.

[0058] Preparation method of modified magnesium hydroxide: According to parts by weight, 3.5 parts of silane coupling agent and 2.5 parts of titanate are dissolved in 50 parts of anhydrous ethanol to form a mixed solution, and then 102 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added to the mixed solution, and dried at 85° C. for 12 hours to obtain modified magnesium hydroxide.

[0059] The silane coupling agent is KH560.

[0060] The flame retardant is red phosphorus.

[0061] The processing aid is prepared by mixing 1 part of polyethylene wax and 4 parts of white oil by weight.

[0062] The antioxidant was BASF Irganox133.

[0063] A method for preparing a flame retardant polyolefin material comprises the following steps:

[0064] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 160°C to obtain a rubber mixture after mixing evenly;

[0065] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0066] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0067] S4: The finished rubber particles can be packaged, tested and put into storage.

[0068] Example 4

[0069] A flame retardant polyolefin material comprises the following components: by weight, 72 parts of high-density polyethylene material, 25 parts of ethylene-vinyl acetate copolymer, 68 parts of modified magnesium hydroxide, 7.5 parts of flame retardant, 5.5 parts of processing aid and 2.2 parts of antioxidant.

[0070] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 27%.

[0071] The preparation method of the modified magnesium hydroxide comprises the following steps: according to parts by weight, 3.2 parts of a silane coupling agent and 2.2 parts of a titanate are dissolved in 46 parts of anhydrous ethanol to form a mixed solution, and then 99 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added into the mixed solution, and dried at 82° C. for 11 hours to obtain the modified magnesium hydroxide.

[0072] The silane coupling agent is KH560.

[0073] The flame retardant is red phosphorus.

[0074] In parts by weight, the processing aid is prepared by mixing 1 part of polyethylene wax and 3.2 parts of white oil.

[0075] The antioxidant is BASF Irganox133.

[0076] A method for preparing a flame retardant polyolefin material comprises the following steps:

[0077] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 135°C to obtain a rubber mixture after mixing evenly;

[0078] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0079] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0080] S4: The finished rubber particles can be packaged, tested and put into storage.

[0081] Example 5

[0082] A flame retardant polyolefin material comprises the following components: by weight, 74 parts of high-density polyethylene material, 28 parts of ethylene-vinyl acetate copolymer, 73 parts of modified magnesium hydroxide, 8.5 parts of flame retardant, 6.5 parts of processing aid and 2.8 parts of antioxidant.

[0083] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 29%.

[0084] Preparation method of modified magnesium hydroxide: According to parts by weight, 3.4 parts of silane coupling agent and 2.4 parts of titanate are dissolved in 48 parts of anhydrous ethanol to form a mixed solution, and then 101 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added to the mixed solution, and dried at 83° C. for 11.2 hours to obtain modified magnesium hydroxide.

[0085] The silane coupling agent is KH550.

[0086] The flame retardant is red phosphorus.

[0087] The processing aid is prepared by mixing 1 part of polyethylene wax and 3.8 parts of white oil by weight.

[0088] The antioxidant was BASF Irganox133.

[0089] A method for preparing a flame retardant polyolefin material comprises the following steps:

[0090] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 155°C to obtain a rubber mixture after mixing evenly;

[0091] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0092] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0093] S4: The finished rubber particles can be packaged, tested and put into storage.

[0094] The difference between Comparative Example 1 and Example 1 is that 25 parts of ethylene-vinyl acetate copolymer are replaced by 15 parts of ethylene-vinyl acetate copolymer.

[0095] A flame retardant polyolefin material comprises the following components: by weight, 75 parts of high-density polyethylene material, 15 parts of ethylene-vinyl acetate copolymer, 70 parts of modified magnesium hydroxide, 8 parts of flame retardant, 6 parts of processing aid and 2.5 parts of antioxidant.

[0096] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in the ethylene-vinyl acetate copolymer is 28%.

[0097] Preparation method of modified magnesium hydroxide: According to parts by weight, 3.5 parts of silane coupling agent and 2.5 parts of titanate are dissolved in 44 parts of anhydrous ethanol to form a mixed solution, and then 100 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added to the mixed solution, and dried at 80° C. for 10 hours to obtain modified magnesium hydroxide.

[0098] The silane coupling agent is KH550.

[0099] The flame retardant is red phosphorus.

[0100] The processing aid is prepared by mixing 1 part of polyethylene wax and 3.5 parts of white oil by weight.

[0101] The antioxidant was BASF Irganox133.

[0102] A method for preparing a flame retardant polyolefin material is as follows:

[0103] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 145°C to obtain a rubber mixture after mixing evenly;

[0104] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0105] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0106] S4: The finished rubber particles can be packaged, tested and put into storage.

[0107] The difference between Comparative Example 2 and Example 1 is that in the preparation of the modified magnesium hydroxide, 3.5 parts of the silane coupling agent are replaced by 3.5 parts of titanate.

[0108] A flame retardant polyolefin material comprises the following components: by weight, 75 parts of high-density polyethylene material, 25 parts of ethylene-vinyl acetate copolymer, 70 parts of modified magnesium hydroxide, 8 parts of flame retardant, 6 parts of processing aid and 2.5 parts of antioxidant.

[0109] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 28%.

[0110] Preparation method of modified magnesium hydroxide: According to parts by weight, 6 parts of titanate are dissolved in 44 parts of anhydrous ethanol to form a mixed solution, and then 100 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added to the mixed solution, and dried at 80° C. for 10 hours to obtain modified magnesium hydroxide.

[0111] The silane coupling agent is KH550.

[0112] The flame retardant is red phosphorus.

[0113] The processing aid is prepared by mixing 1 part of polyethylene wax and 3.5 parts of white oil by weight.

[0114] The antioxidant was BASF Irganox133.

[0115] A method for preparing a flame retardant polyolefin material is as follows:

[0116] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 145°C to obtain a rubber mixture after mixing evenly;

[0117] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0118] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0119] S4: The finished rubber particles can be packaged, tested and put into storage.

[0120] The difference between Comparative Example 3 and Example 1 is that in the preparation of modified magnesium hydroxide, 2.5 parts of titanate are replaced by 2.5 parts of silane coupling agent.

[0121] A flame retardant polyolefin material comprises the following components: by weight, 75 parts of high-density polyethylene material, 25 parts of ethylene-vinyl acetate copolymer, 70 parts of modified magnesium hydroxide, 8 parts of flame retardant, 6 parts of processing aid and 2.5 parts of antioxidant.

[0122] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 28%.

[0123] Preparation method of modified magnesium hydroxide: according to parts by weight, 6 parts of silane coupling agent are dissolved in 44 parts of anhydrous ethanol to form a mixed solution, and then 100 parts of magnesium hydroxide are ground into magnesium hydroxide powder and added into the mixed solution, and dried at 80° C. for 10 hours to obtain modified magnesium hydroxide.

[0124] The flame retardant is red phosphorus.

[0125] The processing aid is prepared by mixing 1 part of polyethylene wax and 3.5 parts of white oil by weight.

[0126] The antioxidant was BASF Irganox133.

[0127] A method for preparing a flame retardant polyolefin material is as follows:

[0128] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 145°C to obtain a rubber mixture after mixing evenly;

[0129] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0130] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0131] S4: The finished rubber particles can be packaged, tested and put into storage.

[0132] The difference between Comparative Example 4 and Example 1 is that in the preparation of the modified magnesium hydroxide, neither silane coupling agent nor titanate is contained.

[0133] A flame retardant polyolefin material comprises the following components: by weight, 75 parts of high-density polyethylene material, 25 parts of ethylene-vinyl acetate copolymer, 70 parts of modified magnesium hydroxide, 8 parts of flame retardant, 6 parts of processing aid and 2.5 parts of antioxidant.

[0134] The high-density polyethylene material is HDPE, and the mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 28%.

[0135] Preparation method of modified magnesium hydroxide: According to parts by weight, 100 parts of magnesium hydroxide are ground into magnesium hydroxide powder and dried at 80° C. for 10 hours to obtain modified magnesium hydroxide.

[0136] The silane coupling agent is KH550.

[0137] The flame retardant is red phosphorus.

[0138] The processing aid is prepared by mixing 1 part of polyethylene wax and 3.5 parts of white oil by weight.

[0139] The antioxidant was BASF Irganox133.

[0140] A method for preparing a flame retardant polyolefin material is as follows:

[0141] S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 145°C to obtain a rubber mixture after mixing evenly;

[0142] S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture;

[0143] S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin;

[0144] S4: The finished rubber particles can be packaged, tested and put into storage.

[0145] The tensile strength of the finished rubber particles is tested in accordance with GB / T2490-2000.

[0146] The fire retardancy of the finished rubber particles is tested with reference to GB / T5464 and GB / T8624.

[0147] The test results are shown in Table 1:

[0148] Table 1

[0149]

[0150]

[0151] Examples 1 to 5 demonstrate that the flame-retardant polyolefin material prepared by the technical solution of the present invention has excellent flame retardant effect and excellent tensile strength.

[0152] The difference between Comparative Example 1 and Example 1 is that 25 parts of ethylene-vinyl acetate copolymer are replaced by 15 parts of ethylene-vinyl acetate copolymer.

[0153] It can be seen from the table that the usage ratio of ethylene-vinyl acetate copolymer to high-density polyethylene affects the tensile strength of the flame-retardant polyolefin material. The usage ratio of ethylene-vinyl acetate copolymer to high-density polyethylene in the technical solution of the present invention can improve the tensile strength of the prepared flame-retardant polyolefin material.

[0154] The difference between Comparative Example 2 and Example 1 is that in the preparation of the modified magnesium hydroxide, 3.5 parts of the silane coupling agent are replaced by 3.5 parts of titanate.

[0155] From the data in Table 1, it can be seen that silane coupling agent can improve the flame retardant properties and tensile strength of flame retardant polyolefin materials.

[0156] The difference between Comparative Example 3 and Example 1 is that in the preparation of modified magnesium hydroxide, 2.5 parts of titanate are replaced by 2.5 parts of silane coupling agent.

[0157] It can be seen from the data in Table 1 that titanate can improve the flame retardant properties and tensile strength of flame retardant polyolefin materials.

[0158] The difference between Comparative Example 4 and Example 1 is that in the preparation of the modified magnesium hydroxide, neither silane coupling agent nor titanate is contained.

[0159] It can be seen from the data in Table 1 that the joint use of silane coupling agent and titanate can synergistically improve the flame retardant properties and tensile strength of flame retardant polyolefin materials.

[0160] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A flame retardant polyolefin material, characterized in that: The invention comprises the following components: by weight, 70-75 parts of high-density polyethylene material, 25-30 parts of ethylene-vinyl acetate copolymer, 65-75 parts of modified magnesium hydroxide, 7-9 parts of flame retardant, 5-7 parts of processing aid and 2-3 parts of antioxidant.

2. The flame retardant polyolefin material according to claim 1, characterized in that: The mass fraction of acetic acid in ethylene-vinyl acetate copolymer is 26-30%.

3. The flame retardant polyolefin material according to claim 1, characterized in that: The preparation method of the modified magnesium hydroxide comprises the following steps: according to parts by weight, 3 to 3.5 parts of a silane coupling agent and 2 to 2.5 parts of a titanate are dissolved in 44 to 50 parts of anhydrous ethanol to form a mixed solution, and then 98 to 102 parts of magnesium hydroxide are ground into magnesium hydroxide powder, added into the mixed solution, and dried at 80 to 85° C. for 10 to 12 hours to obtain the modified magnesium hydroxide.

4. The flame retardant polyolefin material according to claim 3, characterized in that: The silane coupling agent is one of KH550 and KH560 or a mixture of the two in any proportion.

5. The flame retardant polyolefin material according to claim 1, characterized in that: The flame retardant is red phosphorus.

6. The flame retardant polyolefin material according to claim 1, characterized in that: In parts by weight, the processing aid includes 1 part of polyethylene wax and 3 to 4 parts of white oil.

7. The flame retardant polyolefin material according to claim 1, characterized in that: The antioxidant is BASF Irganox133.

8. The method for preparing a flame-retardant polyolefin material according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: Weigh the raw materials of each component by weight, and then put them into an internal mixer, and perform internal mixing and plasticizing at 130-160°C to obtain a rubber mixture after mixing evenly; S2: The rubber mixture enters a two-stage extruder through a conical feeding hopper for shearing, mixing, plasticizing and extrusion, and then granulates by hot cutting on the die surface to obtain a rubber granule mixture; S3: passing the rubber particle mixture through a secondary cyclone separation bin, separating the rubber particles and rubber powder in the rubber particle mixture and cooling it, and then passing it through a vibrating screen to obtain finished rubber particles, which enter a finished product bin; S4: The finished rubber particles can be packaged, tested and put into storage.

Citation Information

Patent Citations

  • Preparation method for halogen-free flame retardant polyethylene waterproof coiled materials

    CN103333428A

  • High-flame-retardant low-smoke, halogen-free and flame-retardant polyolefin tight packing material