Acid and alkali resistant waterproof polyethylene cable and preparation method thereof

By introducing nanohydrotalcite and other components into polyethylene cables, a dense protective layer is formed, which solves the problem of polyethylene cables being easily corroded in acid and alkali environments, significantly improves its acid-base corrosion resistance and waterproof performance, and extends its service life And broadened the application areas.

CN118931016APending Publication Date: 2024-11-12KAIKAI CABLE TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411358731.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing polyethylene cables are prone to corrosion in acid and alkali environments, resulting in reduced performance and shortened service life, and lack effective acid and alkali resistance and waterproofing properties.

Method used

Using nano-hydrtalc to the modification enhancer, combined with polyethylene, crosslinking agent, silicone rubber, inorganic fiber, magnesium hydroxide and zinc oxide, the preparation and extrusion molding process of the modification enhancer is used to form a dense protection. to improve the acid and alkali corrosion resistance of the cable.

Benefits of technology

It significantly improves the acid and alkali corrosion resistance and waterproof properties of polyethylene cables, extends the service life, and broadens its application areas, making it available for long-term use in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064357740000141
    Figure BDA0005064357740000141
  • Figure BDA0005064357740000151
    Figure BDA0005064357740000151
Patent Text Reader

Abstract

The invention discloses an acid-alkali-resistant waterproof polyethylene cable and a preparation method thereof. The acid-alkali-resistant waterproof polyethylene cable comprises a conductor and a sheath, the sheath is prepared from the following components: polyethylene, a cross-linking agent, a modified reinforcing agent, silicone rubber, an anti-aging agent, inorganic fibers, magnesium hydroxide, zinc oxide and a coupling agent; the conductor is a copper core; the polyethylene cable prepared by the invention has excellent mechanical properties, heat resistance, chemical resistance and insulativity, and can be widely applied to the field of power transmission.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cables, in particular to an acid-resistant, alkali-resistant and waterproof polyethylene cable and a preparation method thereof. Background Art

[0002] Waterproof cables play a vital role in the fields of power, communication and construction engineering. Among them, waterproof polyethylene (PE) cables have become the preferred products in many application scenarios due to their unique performance advantages.

[0003] Waterproof polyethylene cable is a special cable made of polyethylene material with excellent cold resistance, corrosion resistance and waterproof performance.

[0004] Since polyethylene material itself has good hydrophobicity, using it as a cable material can effectively prevent moisture from penetrating into the cable and protect the cable's insulation layer and conductor from damage.

[0005] Due to the excellent performance of polyethylene cables, polyethylene cables can be widely used in many fields such as transportation, construction, underground pipelines and power engineering.

[0006] However, although the existing polyethylene cables have good waterproof performance, their acid and alkali corrosion resistance is relatively poor. Long-term exposure to acid and alkali environment can easily cause a significant reduction in cable material performance and significantly shorten the service life of the polyethylene cables.

[0007] Therefore, the present invention solves the corresponding problems by providing an acid-resistant, alkali-resistant and waterproof polyethylene cable. Summary of the invention

[0008] The purpose of the present invention is to provide an acid-resistant and alkali-resistant waterproof polyethylene cable to solve the deficiencies in the prior art.

[0009] The technical solution adopted by the present invention is as follows:

[0010] An acid- and alkali-resistant and waterproof polyethylene cable, comprising a conductor and a sheath;

[0011] The sheath is made of the following ingredients by weight: 90-95 parts of polyethylene, 1-3 parts of cross-linking agent, 15-20 parts of modifying reinforcing agent, 12-16 parts of silicone rubber, 1-1.6 parts of antioxidant, 3-5 parts of inorganic fiber, 6-8 parts of magnesium hydroxide, 1-3 parts of zinc oxide, and 1.5-1.8 parts of coupling agent;

[0012] The conductor is a copper core.

[0013] As a further technical solution: the preparation method of the modified reinforcing agent is:

[0014] First, styrene and maleic anhydride are added into the reactor;

[0015] Adding the initiator to the solvent, stirring and mixing evenly to obtain an initiator solution;

[0016] Inert gas was introduced into the reactor to exhaust the air in the reactor, and then the initiator solution was added into the reactor, the temperature was adjusted to 70° C., and the reaction was stirred for 4 hours under heat preservation, and then the nano-hydrotalcite was added, and the reaction was continued under stirring for 4 hours, and the reaction was terminated to obtain a reaction mixture;

[0017] The reaction mixture is centrifuged, filtered, washed and dried to obtain a modified enhancer;

[0018] Among them, the centrifugal speed is 8000r / min and the time is 15min;

[0019] The drying temperature was 80°C and the drying time was 10 hours.

[0020] As a further technical solution: the molar ratio of styrene to maleic anhydride is 1:1.

[0021] As a further technical solution: the initiator is azobisisobutyronitrile;

[0022] The mass ratio of azobisisobutyronitrile to styrene is 1:200;

[0023] The mixing ratio of azobisisobutyronitrile and solvent is 0.35 g:500 mL;

[0024] The solvent is isoamyl acetate.

[0025] As a further technical solution: the inert gas is nitrogen;

[0026] Based on the total mass of the modified reinforcing agent, the mass fraction of the nano-hydrotalcite is 5-8%.

[0027] As a further technical solution: the preparation method of the nano hydrotalcite is:

[0028] First, magnesium nitrate and aluminum nitrate are added to deionized water respectively, and stirred until dissolved to obtain a mixed solution of magnesium nitrate and aluminum nitrate;

[0029] The molar ratio of magnesium nitrate to aluminum nitrate in the mixed solution of magnesium nitrate and aluminum nitrate is 1:1, and the mass fraction of magnesium nitrate is 12.8%.

[0030] Add sodium hydroxide and sodium carbonate to deionized water respectively, and stir until dissolved to obtain a mixed solution of sodium hydroxide and sodium carbonate;

[0031] The molar ratio of sodium hydroxide to sodium carbonate in the mixed solution of sodium hydroxide and sodium carbonate is 3:1, and the mass fraction of sodium hydroxide is 5.3%.

[0032] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate, and the addition is completed within 30 minutes, and then the stirring is continued for 15 minutes, and then the pH of the reaction system is adjusted to 12, the temperature is adjusted to 120°C, and the mixture is stirred for 12 hours. Then, the material is discharged, centrifuged, filtered, washed to neutrality, and vacuum dried to constant weight to obtain nano hydrotalcite;

[0033] Among them, the centrifugal speed is 5000r / min and the time is 15min;

[0034] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate in a volume ratio of 1:1;

[0035] The reaction system was adjusted using a sodium hydroxide solution with a concentration of 1 mol / L.

[0036] As a further technical solution: the vacuum drying temperature is 50° C. and the vacuum drying time is 20 hours.

[0037] As a further technical solution: the cross-linking agent is silane cross-linking agent A151;

[0038] The antioxidant is antioxidant 4010.

[0039] As a further technical solution: the inorganic fiber is glass fiber;

[0040] The coupling agent is an organic silane coupling agent;

[0041] The organic silane coupling agent is vinyl triethoxy silane.

[0042] A method for preparing an acid-resistant and alkali-resistant waterproof polyethylene cable comprises the following steps:

[0043] S1 Preparation:

[0044] Weigh the following components in parts by weight: polyethylene, crosslinking agent, modifier, silicone rubber, antioxidant, inorganic fiber, magnesium hydroxide, zinc oxide, coupling agent;

[0045] S2 Mixing:

[0046] Add polyethylene, a cross-linking agent, a modifier, a silicone rubber, an antioxidant, an inorganic fiber, magnesium hydroxide, zinc oxide, and a coupling agent into a mixer in sequence, stir and mix, and obtain a mixture;

[0047] S3 conductor installation:

[0048] Pass the conductors through the extruder die in sequence;

[0049] S4 Extrusion Molding:

[0050] The mixed material is added to the extruder for melt extrusion, the conductor is encapsulated with rubber, and then cooled and shaped;

[0051] The temperature of the extruder was set as follows: 135°C in the feeding section, 175°C in the compression section, 180°C in the homogenization section, and 165°C in the die head section;

[0052] The speed of the extruder is set to: 60r / min.

[0053] Beneficial effects:

[0054] The polyethylene cable prepared by the invention has excellent mechanical properties, heat resistance, chemical resistance and insulation, and can be widely used in the field of power transmission.

[0055] In order to improve the corrosion resistance of the polyethylene cable prepared by the present invention, the present invention introduces a prepared modifying and reinforcing agent to greatly improve the corrosion resistance and waterproof performance of the prepared polyethylene cable. The nano hydrotalcite introduced into the modifying and reinforcing agent can significantly enhance the physical and chemical properties of the polyethylene cable due to its extremely high specific surface area and surface energy. In addition, the nano hydrotalcite can not only greatly improve the density of the polyethylene cable in the polyethylene cable, but also form an effective barrier layer to hinder the penetration of corrosive media into the polyethylene cable sheath, thereby greatly improving the acid and alkali corrosion resistance and waterproof performance of the polyethylene cable.

[0056] The invention can greatly improve the dispersibility of nano hydrotalcite particles in polyethylene cables by introducing nano hydrotalcite into the modifying and reinforcing agent, and can form strong physical and chemical effects with polyethylene molecular chains based on the modifying and reinforcing agent, including effects such as hydrogen bonding, van der Waals force or chemical bonding, greatly enhancing the interface interaction, and by greatly enhancing the interface interaction, the overall strength of the prepared polyethylene cable sheath can be significantly improved. Since the modifying and reinforcing agent acts as an intermediary, the nano hydrotalcite can be uniformly dispersed and stably present in the polyethylene cable matrix. When the polyethylene cable is exposed to an acid-base environment, the stable structure can effectively resist the erosion of corrosive media, thereby greatly improving the acid-base corrosion resistance of the polyethylene cable, thereby extending its service life and broadening its application field, so that it can be used for a long time in various complex environments.

[0057] The present invention can form a dense protective layer in the polyethylene cable through the coordination of various components, and this protective layer can block the direct contact of corrosive ions and molecules, thereby slowing down or preventing them from damaging the polyethylene cable substrate. At the same time, the tiny size effect of the nano filler enables it to fill the micropores and defects inside the material, further improving the density and anti-permeability of the material. DETAILED DESCRIPTION

[0058] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0059] The following are specific embodiments

[0060] Example 1

[0061] A method for preparing an acid-resistant and alkali-resistant waterproof polyethylene cable comprises the following steps:

[0062] S1 Preparation:

[0063] Weigh the following according to weight: 90 parts of polyethylene, 11 parts of silane crosslinking agent A15, 15 parts of modifier and reinforcing agent, 12 parts of silicone rubber, 101 parts of antioxidant 40, 3 parts of glass fiber, 6 parts of magnesium hydroxide, 1 part of zinc oxide, and 1.5 parts of vinyl triethoxysilane;

[0064] The conductor is a copper core.

[0065] The preparation method of the modified reinforcing agent is:

[0066] First, styrene and maleic anhydride are added into the reactor;

[0067] Adding azobisisobutyronitrile to isoamyl acetate, stirring and mixing evenly to obtain an azobisisobutyronitrile solution;

[0068] Nitrogen was introduced into the reactor to exhaust the air in the reactor, and then the azobisisobutyronitrile solution was added into the reactor, the temperature was adjusted to 70° C., and the reaction was stirred for 4 hours under heat preservation, and then the nano-hydrotalcite was added, and the reaction was continued under stirring for 4 hours, and the reaction was terminated to obtain a reaction mixture;

[0069] The reaction mixture is centrifuged, filtered, washed and dried to obtain a modified enhancer;

[0070] Among them, the centrifugal speed is 8000r / min and the time is 15min;

[0071] The drying temperature was 80°C and the drying time was 10 hours.

[0072] The molar ratio of styrene to maleic anhydride is 1:1.

[0073] The mass ratio of azobisisobutyronitrile to styrene is 1:200;

[0074] The mixing ratio of azobisisobutyronitrile and solvent is 0.35g:500mL;

[0075] Based on the total mass of the modified reinforcing agent, the mass fraction of the nano-hydrotalcite is 5%.

[0076] The preparation method of nano hydrotalcite is as follows:

[0077] First, magnesium nitrate and aluminum nitrate are added to deionized water respectively, and stirred until dissolved to obtain a mixed solution of magnesium nitrate and aluminum nitrate;

[0078] The molar ratio of magnesium nitrate to aluminum nitrate in the mixed solution of magnesium nitrate and aluminum nitrate is 1:1, and the mass fraction of magnesium nitrate is 12.8%.

[0079] Add sodium hydroxide and sodium carbonate to deionized water respectively, and stir until dissolved to obtain a mixed solution of sodium hydroxide and sodium carbonate;

[0080] The molar ratio of sodium hydroxide to sodium carbonate in the mixed solution of sodium hydroxide and sodium carbonate is 3:1, and the mass fraction of sodium hydroxide is 5.3%.

[0081] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate, and the addition is completed within 30 minutes, and then the stirring is continued for 15 minutes, and then the pH of the reaction system is adjusted to 12, the temperature is adjusted to 120°C, and the mixture is stirred for 12 hours. Then, the material is discharged, centrifuged, filtered, washed to neutrality, and vacuum dried to constant weight to obtain nano hydrotalcite;

[0082] Among them, the centrifugal speed is 5000r / min and the time is 15min;

[0083] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate in a volume ratio of 1:1;

[0084] The reaction system was adjusted using a sodium hydroxide solution with a concentration of 1 mol / L.

[0085] The vacuum drying temperature is 50°C and the vacuum drying time is 20 hours;

[0086] S2 Mixing:

[0087] Add polyethylene, a cross-linking agent, a modifier, a silicone rubber, an antioxidant, an inorganic fiber, magnesium hydroxide, zinc oxide, and a coupling agent into a mixer in sequence, stir and mix, and obtain a mixture;

[0088] S3 conductor installation:

[0089] Pass the conductors through the extruder die in sequence;

[0090] S4 Extrusion Molding:

[0091] The mixed material is added to the extruder for melt extrusion, the conductor is encapsulated with rubber, and then cooled and shaped;

[0092] The temperature of the extruder was set as follows: 135°C in the feeding section, 175°C in the compression section, 180°C in the homogenization section, and 165°C in the die head section;

[0093] The speed of the extruder is set to: 60r / min.

[0094] Example 2

[0095] A method for preparing an acid-resistant and alkali-resistant waterproof polyethylene cable comprises the following steps:

[0096] S1 Preparation:

[0097] Weigh the following according to weight: 92 parts of polyethylene, 12 parts of silane crosslinking agent A15, 16 parts of modifier and reinforcing agent, 13 parts of silicone rubber, 1.2 parts of antioxidant 4010, 3.5 parts of glass fiber, 7 parts of magnesium hydroxide, 2 parts of zinc oxide, and 1.6 parts of vinyl triethoxysilane;

[0098] The conductor is a copper core.

[0099] The preparation method of the modified reinforcing agent is:

[0100] First, styrene and maleic anhydride are added into the reactor;

[0101] Adding azobisisobutyronitrile to isoamyl acetate, stirring and mixing evenly to obtain an azobisisobutyronitrile solution;

[0102] Nitrogen was introduced into the reactor to exhaust the air in the reactor, and then the azobisisobutyronitrile solution was added into the reactor, the temperature was adjusted to 70° C., and the reaction was stirred for 4 hours under heat preservation, and then the nano-hydrotalcite was added, and the reaction was continued under stirring for 4 hours, and the reaction was terminated to obtain a reaction mixture;

[0103] The reaction mixture is centrifuged, filtered, washed and dried to obtain a modified enhancer;

[0104] Among them, the centrifugal speed is 8000r / min and the time is 15min;

[0105] The drying temperature was 80°C and the drying time was 10 hours.

[0106] The molar ratio of styrene to maleic anhydride is 1:1.

[0107] The mass ratio of azobisisobutyronitrile to styrene is 1:200;

[0108] The mixing ratio of azobisisobutyronitrile and solvent is 0.35g:500mL;

[0109] Based on the total mass of the modified reinforcing agent, the mass fraction of the nano-hydrotalcite is 5.5%.

[0110] The preparation method of nano hydrotalcite is as follows:

[0111] First, magnesium nitrate and aluminum nitrate are added to deionized water respectively, and stirred until dissolved to obtain a mixed solution of magnesium nitrate and aluminum nitrate;

[0112] The molar ratio of magnesium nitrate to aluminum nitrate in the mixed solution of magnesium nitrate and aluminum nitrate is 1:1, and the mass fraction of magnesium nitrate is 12.8%.

[0113] Add sodium hydroxide and sodium carbonate to deionized water respectively, and stir until dissolved to obtain a mixed solution of sodium hydroxide and sodium carbonate;

[0114] The molar ratio of sodium hydroxide to sodium carbonate in the mixed solution of sodium hydroxide and sodium carbonate is 3:1, and the mass fraction of sodium hydroxide is 5.3%.

[0115] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate, and the addition is completed within 30 minutes, and then the stirring is continued for 15 minutes, and then the pH of the reaction system is adjusted to 12, the temperature is adjusted to 120°C, and the mixture is stirred for 12 hours. Then, the material is discharged, centrifuged, filtered, washed to neutrality, and vacuum dried to constant weight to obtain nano hydrotalcite;

[0116] Among them, the centrifugal speed is 5000r / min and the time is 15min;

[0117] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate in a volume ratio of 1:1;

[0118] The reaction system was adjusted using a sodium hydroxide solution with a concentration of 1 mol / L.

[0119] The vacuum drying temperature is 50°C and the vacuum drying time is 20 hours;

[0120] S2 Mixing:

[0121] Add polyethylene, a cross-linking agent, a modifier, a silicone rubber, an antioxidant, an inorganic fiber, magnesium hydroxide, zinc oxide, and a coupling agent into a mixer in sequence, stir and mix, and obtain a mixture;

[0122] S3 conductor installation:

[0123] Pass the conductors through the extruder die in sequence;

[0124] S4 Extrusion Molding:

[0125] The mixed material is added to the extruder for melt extrusion, the conductor is encapsulated with rubber, and then cooled and shaped;

[0126] The temperature of the extruder was set as follows: 135°C in the feeding section, 175°C in the compression section, 180°C in the homogenization section, and 165°C in the die head section;

[0127] The speed of the extruder is set to: 60r / min.

[0128] Example 3

[0129] A method for preparing an acid-resistant and alkali-resistant waterproof polyethylene cable comprises the following steps:

[0130] S1 Preparation:

[0131] Weigh the following according to weight: 93 parts of polyethylene, 1512 parts of silane crosslinking agent A, 18 parts of modifier and reinforcing agent, 15 parts of silicone rubber, 1.5 parts of antioxidant 4010, 4 parts of glass fiber, 7 parts of magnesium hydroxide, 2 parts of zinc oxide, and 1.7 parts of vinyl triethoxysilane;

[0132] The conductor is a copper core.

[0133] The preparation method of the modified reinforcing agent is:

[0134] First, styrene and maleic anhydride are added into the reactor;

[0135] Adding azobisisobutyronitrile to isoamyl acetate, stirring and mixing evenly to obtain an azobisisobutyronitrile solution;

[0136] Nitrogen was introduced into the reactor to exhaust the air in the reactor, and then the azobisisobutyronitrile solution was added into the reactor, the temperature was adjusted to 70° C., and the reaction was stirred for 4 hours under heat preservation, and then the nano-hydrotalcite was added, and the reaction was continued under stirring for 4 hours, and the reaction was terminated to obtain a reaction mixture;

[0137] The reaction mixture is centrifuged, filtered, washed and dried to obtain a modified enhancer;

[0138] Among them, the centrifugal speed is 8000r / min and the time is 15min;

[0139] The drying temperature was 80°C and the drying time was 10 hours.

[0140] The molar ratio of styrene to maleic anhydride is 1:1.

[0141] The mass ratio of azobisisobutyronitrile to styrene is 1:200;

[0142] The mixing ratio of azobisisobutyronitrile and solvent is 0.35g:500mL;

[0143] Based on the total mass of the modified reinforcing agent, the mass fraction of the nano-hydrotalcite is 6%.

[0144] The preparation method of nano hydrotalcite is as follows:

[0145] First, magnesium nitrate and aluminum nitrate are added to deionized water respectively, and stirred until dissolved to obtain a mixed solution of magnesium nitrate and aluminum nitrate;

[0146] The molar ratio of magnesium nitrate to aluminum nitrate in the mixed solution of magnesium nitrate and aluminum nitrate is 1:1, and the mass fraction of magnesium nitrate is 12.8%.

[0147] Add sodium hydroxide and sodium carbonate to deionized water respectively, and stir until dissolved to obtain a mixed solution of sodium hydroxide and sodium carbonate;

[0148] The molar ratio of sodium hydroxide to sodium carbonate in the mixed solution of sodium hydroxide and sodium carbonate is 3:1, and the mass fraction of sodium hydroxide is 5.3%.

[0149] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate, and the addition is completed within 30 minutes, and then the stirring is continued for 15 minutes, and then the pH of the reaction system is adjusted to 12, the temperature is adjusted to 120°C, and the mixture is stirred for 12 hours. Then, the material is discharged, centrifuged, filtered, washed to neutrality, and vacuum dried to constant weight to obtain nano hydrotalcite;

[0150] Among them, the centrifugal speed is 5000r / min and the time is 15min;

[0151] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate in a volume ratio of 1:1;

[0152] The reaction system was adjusted using a sodium hydroxide solution with a concentration of 1 mol / L.

[0153] The vacuum drying temperature is 50°C and the vacuum drying time is 20 hours;

[0154] S2 Mixing:

[0155] Add polyethylene, a cross-linking agent, a modifier, a silicone rubber, an antioxidant, an inorganic fiber, magnesium hydroxide, zinc oxide, and a coupling agent into a mixer in sequence, stir and mix, and obtain a mixture;

[0156] S3 conductor installation:

[0157] Pass the conductors through the extruder die in sequence;

[0158] S4 Extrusion Molding:

[0159] The mixed material is added to the extruder for melt extrusion, the conductor is encapsulated with rubber, and then cooled and shaped;

[0160] The temperature of the extruder was set as follows: 135°C in the feeding section, 175°C in the compression section, 180°C in the homogenization section, and 165°C in the die head section;

[0161] The speed of the extruder is set to: 60r / min.

[0162] Example 4

[0163] A method for preparing an acid-resistant and alkali-resistant waterproof polyethylene cable comprises the following steps:

[0164] S1 Preparation:

[0165] Weigh the following according to weight: 94 parts of polyethylene, 12.5 parts of silane crosslinking agent A15, 18 parts of modifier and reinforcing agent, 15 parts of silicone rubber, 1.3 parts of antioxidant 4010, 4 parts of glass fiber, 7 parts of magnesium hydroxide, 2 parts of zinc oxide, and 1.7 parts of vinyl triethoxysilane;

[0166] The conductor is a copper core.

[0167] The preparation method of the modified reinforcing agent is:

[0168] First, styrene and maleic anhydride are added into the reactor;

[0169] Adding azobisisobutyronitrile to isoamyl acetate, stirring and mixing evenly to obtain an azobisisobutyronitrile solution;

[0170] Nitrogen was introduced into the reactor to exhaust the air in the reactor, and then the azobisisobutyronitrile solution was added into the reactor, the temperature was adjusted to 70° C., and the reaction was stirred for 4 hours under heat preservation, and then the nano-hydrotalcite was added, and the reaction was continued under stirring for 4 hours, and the reaction was terminated to obtain a reaction mixture;

[0171] The reaction mixture is centrifuged, filtered, washed and dried to obtain a modified enhancer;

[0172] Among them, the centrifugal speed is 8000r / min and the time is 15min;

[0173] The drying temperature was 80°C and the drying time was 10 hours.

[0174] The molar ratio of styrene to maleic anhydride is 1:1.

[0175] The mass ratio of azobisisobutyronitrile to styrene is 1:200;

[0176] The mixing ratio of azobisisobutyronitrile and solvent is 0.35g:500mL;

[0177] Based on the total mass of the modified reinforcing agent, the mass fraction of the nano-hydrotalcite is 7%.

[0178] The preparation method of nano hydrotalcite is as follows:

[0179] First, magnesium nitrate and aluminum nitrate are added to deionized water respectively, and stirred until dissolved to obtain a mixed solution of magnesium nitrate and aluminum nitrate;

[0180] The molar ratio of magnesium nitrate to aluminum nitrate in the mixed solution of magnesium nitrate and aluminum nitrate is 1:1, and the mass fraction of magnesium nitrate is 12.8%.

[0181] Add sodium hydroxide and sodium carbonate to deionized water respectively, and stir until dissolved to obtain a mixed solution of sodium hydroxide and sodium carbonate;

[0182] The molar ratio of sodium hydroxide to sodium carbonate in the mixed solution of sodium hydroxide and sodium carbonate is 3:1, and the mass fraction of sodium hydroxide is 5.3%.

[0183] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate, and the addition is completed within 30 minutes, and then the stirring is continued for 15 minutes, and then the pH of the reaction system is adjusted to 12, the temperature is adjusted to 120°C, and the mixture is stirred for 12 hours. Then, the material is discharged, centrifuged, filtered, washed to neutrality, and vacuum dried to constant weight to obtain nano hydrotalcite;

[0184] Among them, the centrifugal speed is 5000r / min and the time is 15min;

[0185] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate in a volume ratio of 1:1;

[0186] The reaction system was adjusted using a sodium hydroxide solution with a concentration of 1 mol / L.

[0187] The vacuum drying temperature is 50°C and the vacuum drying time is 20 hours;

[0188] S2 Mixing:

[0189] Add polyethylene, a cross-linking agent, a modifier, a silicone rubber, an antioxidant, an inorganic fiber, magnesium hydroxide, zinc oxide, and a coupling agent into a mixer in sequence, stir and mix, and obtain a mixture;

[0190] S3 conductor installation:

[0191] Pass the conductors through the extruder die in sequence;

[0192] S4 Extrusion Molding:

[0193] The mixed material is added to the extruder for melt extrusion, the conductor is encapsulated with rubber, and then cooled and shaped;

[0194] The temperature of the extruder was set as follows: 135°C in the feeding section, 175°C in the compression section, 180°C in the homogenization section, and 165°C in the die head section;

[0195] The speed of the extruder is set to: 60r / min.

[0196] Example 5

[0197] A method for preparing an acid-resistant and alkali-resistant waterproof polyethylene cable comprises the following steps:

[0198] S1 Preparation:

[0199] Weigh the following according to weight: 95 parts of polyethylene, 13 parts of silane crosslinking agent A15, 20 parts of modifier and reinforcing agent, 16 parts of silicone rubber, 1.6 parts of antioxidant 4010, 5 parts of glass fiber, 8 parts of magnesium hydroxide, 3 parts of zinc oxide, and 1.8 parts of vinyl triethoxysilane;

[0200] The conductor is a copper core.

[0201] The preparation method of the modified reinforcing agent is:

[0202] First, styrene and maleic anhydride are added into the reactor;

[0203] Adding azobisisobutyronitrile to isoamyl acetate, stirring and mixing evenly to obtain an azobisisobutyronitrile solution;

[0204] Nitrogen was introduced into the reactor to exhaust the air in the reactor, and then the azobisisobutyronitrile solution was added into the reactor, the temperature was adjusted to 70° C., and the reaction was stirred for 4 hours under heat preservation, and then the nano-hydrotalcite was added, and the reaction was continued under stirring for 4 hours, and the reaction was terminated to obtain a reaction mixture;

[0205] The reaction mixture is centrifuged, filtered, washed and dried to obtain a modified enhancer;

[0206] Among them, the centrifugal speed is 8000r / min and the time is 15min;

[0207] The drying temperature was 80°C and the drying time was 10 hours.

[0208] The molar ratio of styrene to maleic anhydride is 1:1.

[0209] The mass ratio of azobisisobutyronitrile to styrene is 1:200;

[0210] The mixing ratio of azobisisobutyronitrile and solvent is 0.35g:500mL;

[0211] Based on the total mass of the modified reinforcing agent, the mass fraction of the nano-hydrotalcite is 8%.

[0212] The preparation method of nano hydrotalcite is as follows:

[0213] First, magnesium nitrate and aluminum nitrate are added to deionized water respectively, and stirred until dissolved to obtain a mixed solution of magnesium nitrate and aluminum nitrate;

[0214] The molar ratio of magnesium nitrate to aluminum nitrate in the mixed solution of magnesium nitrate and aluminum nitrate is 1:1, and the mass fraction of magnesium nitrate is 12.8%.

[0215] Add sodium hydroxide and sodium carbonate to deionized water respectively, and stir until dissolved to obtain a mixed solution of sodium hydroxide and sodium carbonate;

[0216] The molar ratio of sodium hydroxide to sodium carbonate in the mixed solution of sodium hydroxide and sodium carbonate is 3:1, and the mass fraction of sodium hydroxide is 5.3%.

[0217] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate, and the addition is completed within 30 minutes, and then the stirring is continued for 15 minutes, and then the pH of the reaction system is adjusted to 12, the temperature is adjusted to 120°C, and the mixture is stirred for 12 hours. Then, the material is discharged, centrifuged, filtered, washed to neutrality, and vacuum dried to constant weight to obtain nano hydrotalcite;

[0218] Among them, the centrifugal speed is 5000r / min and the time is 15min;

[0219] The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate in a volume ratio of 1:1;

[0220] The reaction system was adjusted using a sodium hydroxide solution with a concentration of 1 mol / L.

[0221] The vacuum drying temperature is 50°C and the vacuum drying time is 20 hours;

[0222] S2 Mixing:

[0223] Add polyethylene, a cross-linking agent, a modifier, a silicone rubber, an antioxidant, an inorganic fiber, magnesium hydroxide, zinc oxide, and a coupling agent into a mixer in sequence, stir and mix, and obtain a mixture;

[0224] S3 conductor installation:

[0225] Pass the conductors through the extruder die in sequence;

[0226] S4 Extrusion Molding:

[0227] The mixed material is added to the extruder for melt extrusion, the conductor is encapsulated with rubber, and then cooled and shaped;

[0228] The temperature of the extruder was set as follows: 135°C in the feeding section, 175°C in the compression section, 180°C in the homogenization section, and 165°C in the die head section;

[0229] The speed of the extruder is set to: 60r / min.

[0230] Comparative Example 1:

[0231] Based on the technical solution of Example 1, the difference from the technical solution of Example 1 is that no modifying enhancer is added.

[0232] Comparative Example 2:

[0233] On the basis of the technical solution of Example 1, the difference from the technical solution of Example 1 is that the modifying reinforcing agent is replaced with an equal amount of nano-hydrotalcite contained therein.

[0234] test:

[0235] Dielectric properties: The sheath samples of the embodiment were tested using a Concept80 broadband dielectric and impedance spectrometer. The test conditions were 0.1 Hz and the test temperature was 20°C. The relative dielectric constant and conductivity were tested:

[0236] Table 1

[0237] <![CDATA[Conductivity × 10 -16 S / cm]]> Dielectric constant Example 1 1.60 2.26 Example 2 1.65 2.20 Example 3 1.63 2.24 Example 4 1.61 2.22 Example 5 1.66 2.23

[0238] It can be seen from Table 2 that the sheath material of the polyethylene cable prepared in the present invention has excellent dielectric properties.

[0239] According to the standard GB1040-79, the tensile strength of the sheath samples of the embodiment and the comparative example is tested:

[0240] Table 2

[0241] Tensile strength at break MPa Example 1 23.26 Example 2 23.89 Example 3 24.05 Example 4 23.77 Example 5 23.51 Comparative Example 1 20.05 Comparative Example 2 20.98

[0242] It can be seen from Table 2 that the polyethylene cable prepared in the present invention has excellent tensile strength at break.

[0243] Acid corrosion resistance test: The sheath samples of the embodiment and the comparative example were immersed in a 5% sulfuric acid solution at room temperature for 100 hours, then taken out, washed to neutrality, dried, and tested for tensile breaking strength;

[0244] Table 3

[0245] Tensile strength at break MPa Example 1 22.66 Example 2 22.93 Example 3 23.05 Example 4 22.78 Example 5 22.80 Comparative Example 1 17.14 Comparative Example 2 18.85

[0246] It can be seen from Table 3 that the polyethylene cable prepared by the present invention has excellent acid corrosion resistance.

[0247] Alkali corrosion resistance test: The sheath samples of the embodiment and the comparative example were immersed in 10% sodium hydroxide solution at room temperature for 100 hours, then taken out, washed to neutrality, dried, and tested for tensile strength.

[0248] Table 4

[0249]

[0250]

[0251] It can be seen from Table 4 that the polyethylene cable prepared in the present invention has excellent alkali corrosion resistance.

[0252] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. An acid- and alkali-resistant and waterproof polyethylene cable, characterized in that: Including conductor and sheath; The sheath is made of the following ingredients by weight: 90-95 parts of polyethylene, 1-3 parts of cross-linking agent, 15-20 parts of modifying reinforcing agent, 12-16 parts of silicone rubber, 1-1.6 parts of antioxidant, 3-5 parts of inorganic fiber, 6-8 parts of magnesium hydroxide, 1-3 parts of zinc oxide, and 1.5-1.8 parts of coupling agent; The conductor is a copper core.

2. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 1, characterized in that: The preparation method of the modified reinforcing agent is: First, styrene and maleic anhydride are added into the reactor; Adding the initiator to the solvent, stirring and mixing evenly to obtain an initiator solution; Inert gas was introduced into the reactor to exhaust the air in the reactor, and then the initiator solution was added into the reactor, the temperature was adjusted to 70° C., and the reaction was stirred for 4 hours under heat preservation, and then the nano-hydrotalcite was added, and the reaction was continued under stirring for 4 hours, and the reaction was terminated to obtain a reaction mixture; The reaction mixture is centrifuged, filtered, washed and dried to obtain a modified enhancer; Among them, the centrifugal speed is 8000r / min and the time is 15min; The drying temperature was 80°C and the drying time was 10 hours.

3. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 2, characterized in that: The molar ratio of styrene to maleic anhydride is 1:

1.

4. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 2, characterized in that: The initiator is azobisisobutyronitrile; The mass ratio of azobisisobutyronitrile to styrene is 1:200; The mixing ratio of azobisisobutyronitrile and solvent is 0.35 g:500 mL; The solvent is isoamyl acetate.

5. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 2, characterized in that: The inert gas is nitrogen; Based on the total mass of the modified reinforcing agent, the mass fraction of the nano-hydrotalcite is 5-8%.

6. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 5, characterized in that: The nano hydrotalcite preparation method is: First, magnesium nitrate and aluminum nitrate are added to deionized water respectively, and stirred until dissolved to obtain a mixed solution of magnesium nitrate and aluminum nitrate; The molar ratio of magnesium nitrate to aluminum nitrate in the mixed solution of magnesium nitrate and aluminum nitrate is 1:1, and the mass fraction of magnesium nitrate is 12.8%. Add sodium hydroxide and sodium carbonate to deionized water respectively, and stir until dissolved to obtain a mixed solution of sodium hydroxide and sodium carbonate; The molar ratio of sodium hydroxide to sodium carbonate in the mixed solution of sodium hydroxide and sodium carbonate is 3:1, and the mass fraction of sodium hydroxide is 5.3%. The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate, and the addition is completed within 30 minutes, and then the stirring is continued for 15 minutes, and then the pH of the reaction system is adjusted to 12, the temperature is adjusted to 120°C, and the mixture is stirred for 12 hours. Then, the material is discharged, centrifuged, filtered, washed to neutrality, and vacuum dried to constant weight to obtain nano hydrotalcite; Among them, the centrifugal speed is 5000r / min and the time is 15min; The mixed solution of sodium hydroxide and sodium carbonate is added dropwise to the mixed solution of magnesium nitrate and aluminum nitrate in a volume ratio of 1:1; The reaction system was regulated using a sodium hydroxide solution with a concentration of 1 mol / L.

7. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 6, characterized in that: The vacuum drying temperature is 50° C., and the vacuum drying time is 20 hours.

8. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 1, characterized in that: The crosslinking agent is silane crosslinking agent A151; The antioxidant is antioxidant 4010.

9. The acid- and alkali-resistant and waterproof polyethylene cable according to claim 1, characterized in that: The inorganic fiber is glass fiber; The coupling agent is an organic silane coupling agent; The organic silane coupling agent is vinyl triethoxy silane.

10. The method for preparing an acid- and alkali-resistant and waterproof polyethylene cable according to claim 1, characterized in that: The following steps are involved: S1 Preparation: Weigh the following components in parts by weight: polyethylene, crosslinking agent, modifier, silicone rubber, antioxidant, inorganic fiber, magnesium hydroxide, zinc oxide, coupling agent; S2 Mixing: Add polyethylene, a cross-linking agent, a modifier, a silicone rubber, an antioxidant, an inorganic fiber, magnesium hydroxide, zinc oxide, and a coupling agent into a mixer in sequence, stir and mix, and obtain a mixture; S3 conductor installation: Pass the conductors through the extruder die in sequence; S4 Extrusion Molding: The mixed material is added to the extruder for melt extrusion, the conductor is encapsulated with rubber, and then cooled and shaped; The temperature of the extruder was set as follows: 135°C in the feeding section, 175°C in the compression section, 180°C in the homogenization section, and 165°C in the die head section; The speed of the extruder is set to: 60r / min.

Citation Information

Patent Citations

  • Preparation method for halogen-free flame retardant polyethylene waterproof coiled materials

    CN103333428A

  • Preparation method of poly nano silicon dioxide magnesium aluminum borate hydrotalcite

    CN104556083A

  • High-strength wear-resistant submarine cable outer sheath material

    CN105623052A

  • Modified hydrotalcite, as well as preparation method and application thereof in processing of polyvinyl chloride

    CN106188929A

  • Special protective casing for computer cable and production process of special protective casing

    CN106633308A