Antibacterial permanent antistatic composite material applied to foaming shoe material and preparation method

By using modified nanosilver particles and ellowite nanotubes in foamed shoe materials, combined with raw materials such as ethylene-vinyl acetate copolymers, a composite material with excellent antibacterial and antistatic properties was prepared, and the existing solutions were solved The problem of insufficient rebound performance of shoe materials has achieved effective performance of the lightweight, high elasticity and shock absorption functions of EVA materials.

CN118931020APending Publication Date: 2024-11-12GUANGDONG GERUI NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411006663.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing foamed shoe materials lack excellent antibacterial and antistatic properties, and lack of rebound performance, so they cannot effectively exert the lightweight, high elasticity and shock absorption functions of EVA materials.

Method used

Using ethylene-vinyl acetate copolymer, polystyrene-polybutadiene-polystyrene triblock copolymer, nano-calcium carbonate, polyaniline modified Elosite nanotubes, 4,4-oxodiphenylsulfonium sulfonium Raw materials such as hydrazide, grafted modified nanosilver particles and diisopropyl peroxide are prepared by melting and mixing of twin-screw extruders, and the modification of nanosilver particles and eloite nanotubes is improved. Dispersibility and performance.

Benefits of technology

It realizes the excellent antibacterial and antistatic properties of foamed shoes, and improves the rebound performance, effectively exerting the lightweight, high elasticity and shock absorption functions of EVA materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963183070000091
    Figure BDA0004963183070000091
Patent Text Reader

Abstract

The invention discloses an antibacterial permanent antistatic composite material applied to a foamed shoe material, which is prepared from the following raw materials: 50-70 parts of ethylene-vinyl acetate copolymer, 10-20 parts of polystyrene-polybutadiene-polystyrene triblock copolymer, 10-20 parts of nano calcium carbonate, 3-6 parts of polyaniline modified halloysite nanotube, 3-6 parts of 4, 4 '-diphenyl-1, 3-pentanediol monoisobutyrate, 1-3 parts of sodium dodecyl benzene sulfonate, 1-3 parts of sodium dodecyl benzene sulfonate, the coating is prepared from the following components in parts by weight: 2-3 parts of 2, 4-oxo-dibenzenesulfonyl hydrazide, 1-2 parts of grafted modified nano-silver particles, 0.7-1.2 parts of dicumyl peroxide and 0.4-1 part of an anti-aging agent. The antibacterial and antistatic composite material has excellent antibacterial and antistatic properties; meanwhile, the rebound resilience of the foaming shoe material is also improved, and the functions of light weight, high elasticity and shock absorption of EVA are effectively exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer composite materials, and in particular to an antibacterial permanent antistatic composite material used for foaming shoe materials and a preparation method thereof. Background Art

[0002] Ethylene-vinyl acetate copolymer (EVA) is made by copolymerization of ethylene (E) and vinyl acetate (VA), and the general vinyl acetate (VA) content is 5% to 40%; due to the introduction of vinyl acetate monomer into the molecular chain, the crystallinity is reduced, and the flexibility, impact resistance, filler compatibility and heat sealing performance are improved. EVA foaming materials are widely used in many fields such as automobiles, electrical appliances, sole materials, and building thermal insulation materials. For EVA composite materials, the performance is usually improved by two aspects: the synthesis of EVA materials, grafting modification, etc., and the compounding of composite materials.

[0003] Patent CN 113024960 A discloses a heat-resistant, wear-resistant, high-strength modified EVA rubber-plastic foam material and a preparation method. The components of the modified EVA rubber-plastic foam material include modified EVA resin, polypropylene, polyurethane, natural rubber, carboxylated zinc oxide whisker, foaming agent, stearic acid, antioxidant, diisopropylbenzene peroxide and aziridine crosslinking agent. Among them, the modified EVA resin is prepared by first reacting the EVA resin with sodium hydroxide in a molten state and then reacting with bis(carboxylphthalimide). The present invention modifies EVA, introduces benzene rings, imide groups and carboxyl groups on its side groups, and performs carboxyl modification on the filler zinc oxide whisker, and simultaneously uses diisopropylbenzene peroxide and aziridine crosslinking agent in combination, and after mixing and hot pressing foaming, the heat resistance, wear resistance and strength of the EVA rubber-plastic foam material are improved.

[0004] Patent CN 109912877 A discloses a high temperature resistant and anti-aging EVA foam material and its preparation method and application. The foam material is made by foaming an EVA composite material, and the EVA composite material includes: 40-50 parts of EVA; 10-55 parts of AEM rubber; 10-20 parts of polyolefin elastomer; 10-20 parts of ethylene octene block copolymer; 0.5-0.8 parts of peroxide crosslinking agent; 3-5 parts of foaming agent; 1-4 parts of active agent; 3-12 parts of reinforcing agent. The thermal shrinkage rate of the foam material is 0.6-1%, which is lower than the thermal shrinkage rate of traditional EVA foam materials. After aging in hot air, the permanent compression deformation change rate, mechanical property change rate and hardness change rate of the foam material are all less than 20%, which well maintains the original performance of the material and has good high temperature resistance and anti-aging properties.

[0005] Patent CN 109233178 A discloses ultra-light shock-absorbing and wear-resistant foamed shoe material and its manufacturing method, which is composed of 0% to 30% ethylene-vinyl acetate copolymer, 37% to 68% polymer polyol, 10% to 20% polyolefin block copolymer, 5% to 15% ethylene-acrylic acid copolymer, 5% to 10% anti-wear agent, 3% to 8% talcum powder, 0.2% to 0.6% stearic acid, 0.3% to 1.0% zinc stearate, 1.0% to 2.0% zinc oxide, 0.4% to 0.6% di-(tert-butylperoxyisopropyl)benzene, 4% to 6% azodicarbonamide, 2% to 3% masterbatch, and the total mass is 100%. The prepared ultra-light shock-absorbing and wear-resistant foamed shoe material not only achieves ultra-light, shock-absorbing and comfortable performance, but also meets the requirements of wear resistance and wear resistance.

[0006] Patent CN 103450545 A discloses an antistatic sole material for a clean room, which is composed of the following materials in parts by weight: 76 to 80 parts of ethylene-vinyl acetate copolymer particles, 4 to 5 parts of bridging agents, 1.2 to 1.5 parts of bridging aids, 9 to 11 parts of calcium carbonate, 2.5 to 3 parts of azodicarbonamide powder, 1.2 to 1.3 parts of dicumyl peroxide powder, 1.6 to 1.7 parts of zinc oxide powder, 1.2 to 1.3 parts of stearic acid powder, 3 to 6 parts of alkylphenol polyoxyethylene ether liquid, 3 to 6 parts of stearamidopropyl dimethyl-b-hydroxyethyl ammonium nitrate liquid, 0.5 to 1.5 parts of glyceryl monostearate particles, 0.5 to 1.5 parts of ethoxylated alkyl ammonium sulfate solids, and 0.5 to 1.5 parts of ethoxylated alcohol solids.

[0007] For foamed shoe materials, good antibacterial properties need to be considered; for special working environments, there are clear requirements for antistatic performance; giving foamed shoe materials antibacterial and antistatic properties is one of the directions pursued and researched by existing shoe factories. Summary of the invention

[0008] Based on the deficiencies and needs of the prior art, the purpose of the present invention is to provide an antibacterial and permanent antistatic composite material for foamed shoe materials and a preparation method thereof, so that the composite material has excellent antibacterial and antistatic properties; at the same time, the rebound performance of the foamed shoe material is also improved, and the light weight, high elasticity and shock absorption functions of EVA are effectively exerted.

[0009] In order to solve the technical problem of the present invention, the following specific technical solution is adopted:

[0010] An antibacterial and permanent antistatic composite material for foamed shoe materials, comprising the following raw materials in parts by weight:

[0011] 50-70 parts of ethylene-vinyl acetate copolymer,

[0012] 10-20 parts of polystyrene-polybutadiene-polystyrene triblock copolymer,

[0013] 10-20 parts of nano calcium carbonate (nucleating agent, filler)

[0014] 3-6 parts of polyaniline modified halloysite nanotubes (antistatic)

[0015] 2-3 parts of 4,4-oxydibenzenesulfonylhydrazide (foaming agent)

[0016] Graft modified nano silver particles 1-2 parts,

[0017] 0.7-1.2 parts of dicumyl peroxide,

[0018] Anti-aging agent 0.4 to 1 part.

[0019] Furthermore, the composition includes the following raw materials in parts by weight:

[0020] 55-65 parts of ethylene-vinyl acetate copolymer,

[0021] 13-16 parts of polystyrene-polybutadiene-polystyrene triblock copolymer,

[0022] 12-17 parts of nano calcium carbonate (nucleating agent, filler)

[0023] 4-5 parts of polyaniline modified halloysite nanotubes (antistatic)

[0024] 2-2.5 parts of 4,4-oxydibenzenesulfonylhydrazide (foaming agent)

[0025] Graft modified nano silver particles 1.5-2 parts,

[0026] 0.9-1.1 parts of dicumyl peroxide,

[0027] Anti-aging agent 0.6-0.8 parts.

[0028] Further, it is composed of the following raw materials in parts by weight:

[0029] 55-65 parts of ethylene-vinyl acetate copolymer,

[0030] 13-16 parts of polystyrene-polybutadiene-polystyrene triblock copolymer,

[0031] 12-17 parts of nano calcium carbonate (nucleating agent, filler)

[0032] 4-5 parts of polyaniline modified halloysite nanotubes (antistatic)

[0033] 2-2.5 parts of 4,4-oxydibenzenesulfonylhydrazide (foaming agent)

[0034] Graft modified nano silver particles 1.5-2 parts,

[0035] 0.9-1.1 parts of dicumyl peroxide,

[0036] Anti-aging agent 0.6-0.8 parts.

[0037] Furthermore, the particle size of the nano calcium carbonate is 400-500 nm.

[0038] Furthermore, the anti-aging agent is selected from ethoxyquinoline or N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine.

[0039] In the prior art, halloysite is also widely used as a flame retardant component in foamed composite materials. In addition, halloysite grafted with conductive polymers can play an antistatic role. The present invention pre-grafts the conductive polymer polyaniline on the halloysite nanotubes, which not only utilizes the flame retardancy of halloysite but also plays its antistatic role, without the need to add an additional antistatic agent. In addition, after the grafting of polyaniline, the dispersibility problem of the halloysite nanotubes in the ethylene-vinyl acetate copolymer matrix is ​​also solved.

[0040] Furthermore, the preparation method of the polyaniline modified halloysite nanotubes is:

[0041] (1) Add 100 parts of water to a reaction container, then add 1.5 to 3.5 parts of dodecyldimethylsulfonyl betaine, turn on the stirring device to mix evenly; turn on the heater to raise the solution temperature to 50 to 60° C., then add 20 to 30 parts of halloysite nanotubes, and continue stirring for 10 to 20 minutes;

[0042] (2) Add dilute hydrochloric acid to the reactor, stop adding when the pH reaches 4.6 to 4.7, and place the reactor in an ice bath at -5 to 0°C to wait for the solution temperature to stabilize;

[0043] (3) adding 5 to 10 parts of aniline monomer to the reactor, controlling the stirring rate to 10 to 15 rpm, and applying ultrasound during the stirring process; then dripping 3 to 5 parts of ammonium persulfate solution into the reactor, wherein the dripping time is controlled to be 20 to 30 minutes;

[0044] (4) The reaction solution of step (3) is filtered and washed with anhydrous ethanol and deionized water for 2 to 3 times, and the solid component is placed in a drying oven for drying to obtain polyaniline-modified halloysite nanotubes.

[0045] In the present application, nano calcium carbonate is added, which can be used as a filler and a nucleating agent, and can fill and modify ethylene-vinyl acetate copolymer, thereby improving its hardness and resilience; in addition, by adding a nucleating agent, the crystallization behavior and crystal structure of EVA can be controlled, thereby improving its resilience. By adding a nucleating agent, the crystallization behavior and crystal structure of EVA can be controlled, thereby improving its resilience.

[0046] In the present application, nano silver particles are used as antibacterial agents. However, the simple use of nano silver particles has the defect of poor dispersibility. Therefore, the present application performs surface grafting modification on the nano silver particles to improve their dispersibility in the ethylene-vinyl acetate copolymer matrix. On the other hand, although most of the surface modification methods of nano silver particles can improve dispersibility, their antibacterial properties are obviously inferior to those of simple nano silver particles. Based on the above considerations, the applicant seeks a modification method that can improve dispersibility without reducing antibacterial properties.

[0047] Furthermore, the preparation steps of the grafted modified nano silver particles are as follows: (1) tetrahydrofuran and water are mixed in a volume ratio of 1:2 in a reactor to form a 1L solution, 20-30g of silver particles with a particle size of 200nm are added thereto, and an inert gas is flushed into the reactor; 0.5-1g of 2-butyl-6-phenylpyridine is added and stirred continuously;

[0048] (2) raising the temperature of the reactor to 50-60° C., adding 0.1-0.2 g of azobisisobutyronitrile and reacting for 5-7 hours; (3) lowering the temperature to room temperature after the reaction, stopping the introduction of inert gas and stopping stirring; filtering the reaction solution, washing with anhydrous ethanol and deionized water in turn; and drying to obtain grafted modified nanosilver particles.

[0049] A method for preparing an antibacterial permanent antistatic composite material for foamed shoe materials comprises the following steps:

[0050] (1) Weigh the components in proportion for later use;

[0051] (2) Pour ethylene-vinyl acetate copolymer, graft-modified, polyaniline-modified halloysite nanotubes, and 4,4-oxydibenzenesulfonyl hydrazide into a stirring device according to weight parts and stir evenly to form material group A; pour polystyrene-polybutadiene-polystyrene triblock copolymer, nano-calcium carbonate, dicumyl peroxide, and an anti-aging agent into a stirring device according to weight parts and stir evenly to form material group B;

[0052] (3) Material group A is fed from the main feed of a twin-screw extruder, and material group B is fed from the side feed of the twin-screw extruder, and the mixture is melted, mixed, and extruded through the twin-screw extruder to obtain a polycarbonate composite material.

[0053] Furthermore, the set temperature of the twin-screw extruder is: section one: 165-175°C, section two: 170-180°C, section three: 175-185°C, section four: 180-190°C, section five: 165-175°C, section six: 170-180°C, section seven: 170-180°C, section eight: 170-180°C, section nine: 175-185°C, and die head: 180-190°C.

[0054] Furthermore, the rotation speed of the twin-screw extruder is 200-250 rpm.

[0055] The antibacterial permanent antistatic composite material for foamed shoe materials and the preparation method thereof provided by the present invention have the following beneficial effects compared with the prior art:

[0056] (1) The present invention has developed an antibacterial and permanent antistatic composite material for foamed shoe materials through research on raw materials. The composite material has excellent antibacterial and antistatic properties. At the same time, the rebound performance of the foamed shoe materials is also improved, and the light weight, high elasticity and shock absorption functions of EVA are effectively brought into play.

[0057] (2) The present invention improves the dispersibility of nanosilver particles in the polystyrene-polybutadiene-polystyrene triblock copolymer matrix by surface grafting modification without reducing the antibacterial property.

[0058] (3) The polyaniline-modified halloysite nanotubes of the present invention achieve permanent antistatic properties of the composite material and also solve the problem of the dispersibility of the halloysite nanotubes in the ethylene-vinyl acetate copolymer matrix. DETAILED DESCRIPTION

[0059] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0060] Main raw materials: Ethylene-vinyl acetate copolymer is the product UL 7711 of Exxon Corporation of the United States; polystyrene-polybutadiene-polystyrene triblock copolymer (SBS) is the product 4452 of Sinopec Corporation.

[0061] The preparation method of polyaniline modified halloysite nanotubes is as follows:

[0062] (1) Add 100 parts of water to a reaction container, then add 2 parts of dodecyldimethylsulfonyl betaine, turn on the stirring device to mix evenly; turn on the heater to raise the solution temperature to 53° C., then add 25 parts of halloysite nanotubes, and continue stirring for 15 minutes;

[0063] (2) Add dilute hydrochloric acid to the reactor, stop adding when the pH reaches 4.6, and place the reactor in an ice bath at -5°C until the solution temperature stabilizes;

[0064] (3) adding 7 parts of aniline monomer to the reactor, controlling the stirring rate at 10 rpm, and applying ultrasound during the stirring process; then dropping 4 parts of ammonium persulfate solution into the reactor, wherein the dropping time is controlled to be 25 min;

[0065] (4) The reaction solution of step (3) is filtered and washed with anhydrous ethanol and deionized water for three times, and the solid component is placed in a drying oven for drying to obtain polyaniline-modified halloysite nanotubes.

[0066] The preparation steps of grafted modified nano silver particles are as follows: (1) tetrahydrofuran and water are mixed in a volume ratio of 1:2 in a reactor to form a 1L solution, 25g of silver particles with a particle size of 200nm are added thereto, and inert gas N2 is flushed into the reactor; 0.7g of 2-butyl-6-phenylpyridine is added and stirred continuously;

[0067] (2) Raise the temperature of the reactor to 55°C, add 0.15 g of azobisisobutyronitrile and react for 6 hours;

[0068] (3) After the reaction is completed, the temperature is lowered to room temperature, the inert gas is stopped, and the stirring is stopped; the reaction solution is filtered, washed with anhydrous ethanol and deionized water in sequence; and dried to obtain the grafted modified nanosilver particles.

[0069] In the following examples and comparative examples, the raw materials used were those mentioned above unless otherwise specified.

[0070] Example 1

[0071] An antibacterial and permanent antistatic composite material for foamed shoe materials, comprising the following raw materials in parts by weight:

[0072] 55 parts of ethylene-vinyl acetate copolymer,

[0073] 13 parts of polystyrene-polybutadiene-polystyrene triblock copolymer,

[0074] 12 parts of nano calcium carbonate,

[0075] 4 parts of polyaniline modified halloysite nanotubes,

[0076] 2 parts of 4,4-oxydibenzenesulfonyl hydrazide,

[0077] Graft modified nano silver particles 1.5 parts,

[0078] 0.9 parts of dicumyl peroxide,

[0079] Anti-aging agent 0.6 parts.

[0080] Among them, the particle size of nano calcium carbonate is 400nm.

[0081] Wherein, the anti-aging agent is selected from ethoxyquinoline.

[0082] A method for preparing an antibacterial permanent antistatic composite material for foamed shoe materials comprises the following steps:

[0083] (1) Weigh the components in proportion for later use;

[0084] (2) Pour ethylene-vinyl acetate copolymer, graft-modified, polyaniline-modified halloysite nanotubes, and 4,4-oxydibenzenesulfonyl hydrazide into a stirring device according to weight parts and stir evenly to form material group A; pour polystyrene-polybutadiene-polystyrene triblock copolymer, nano-calcium carbonate, dicumyl peroxide, and an anti-aging agent into a stirring device according to weight parts and stir evenly to form material group B;

[0085] (3) Material group A is fed from the main feed of a twin-screw extruder, and material group B is fed from the side feed of the twin-screw extruder, and the mixture is melted, mixed, and extruded through the twin-screw extruder to obtain a polycarbonate composite material.

[0086] Among them, the set temperatures of the twin-screw extruder are: section one: 165°C, section two: 170°C, section three: 175°C, section four: 180°C, section five: 165°C, section six: 170°C, section seven: 170°C, section eight: 170°C, section nine: 175°C, and die head: 180°C.

[0087] Among them, the rotation speed of the twin-screw extruder is 200 rpm.

[0088] Example 2

[0089] An antibacterial and permanent antistatic composite material for foamed shoe materials, comprising the following raw materials in parts by weight:

[0090] 65 parts of ethylene-vinyl acetate copolymer,

[0091] 16 parts of polystyrene-polybutadiene-polystyrene triblock copolymer,

[0092] 17 parts of nano calcium carbonate,

[0093] 5 parts of polyaniline modified halloysite nanotubes,

[0094] 2.5 parts of 4,4-oxydibenzenesulfonylhydrazide,

[0095] Graft modified nano silver particles 2 parts,

[0096] 1.1 parts of dicumyl peroxide,

[0097] Anti-aging agent 0.8 parts.

[0098] Among them, the particle size of nano calcium carbonate is 500nm.

[0099] Wherein, the anti-aging agent is selected from N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine.

[0100] A method for preparing an antibacterial permanent antistatic composite material for foamed shoe materials comprises the following steps:

[0101] (1) Weigh the components in proportion for later use;

[0102] (2) Pour ethylene-vinyl acetate copolymer, graft-modified, polyaniline-modified halloysite nanotubes, and 4,4-oxydibenzenesulfonyl hydrazide into a stirring device according to weight parts and stir evenly to form material group A; pour polystyrene-polybutadiene-polystyrene triblock copolymer, nano-calcium carbonate, dicumyl peroxide, and an anti-aging agent into a stirring device according to weight parts and stir evenly to form material group B;

[0103] (3) Material group A is fed from the main feed of a twin-screw extruder, and material group B is fed from the side feed of the twin-screw extruder, and the mixture is melted, mixed, and extruded through the twin-screw extruder to obtain a polycarbonate composite material.

[0104] Among them, the set temperatures of the twin-screw extruder are: section one: 175°C, section two: 180°C, section three: 185°C, section four: 190°C, section five: 175°C, section six: 180°C, section seven: 180°C, section eight: 180°C, section nine: 185°C, and die head: 190°C.

[0105] Wherein, the rotation speed of the twin-screw extruder is 250 rpm.

[0106] Example 3

[0107] An antibacterial and permanent antistatic composite material for foamed shoe materials, comprising the following raw materials in parts by weight:

[0108] 60 parts of ethylene-vinyl acetate copolymer,

[0109] 15 parts of polystyrene-polybutadiene-polystyrene triblock copolymer,

[0110] 14 parts of nano calcium carbonate (nucleating agent, filler)

[0111] 4.5 parts of polyaniline modified halloysite nanotubes (antistatic)

[0112] 23 parts of 4,4-oxydibenzenesulfonylhydrazide (foaming agent)

[0113] 1.8 parts of grafted modified nano silver particles,

[0114] 1 part dicumyl peroxide,

[0115] Anti-aging agent 0.7 parts.

[0116] Among them, the particle size of nano calcium carbonate is 450nm.

[0117] Wherein, the anti-aging agent is selected from ethoxyquinoline.

[0118] A method for preparing an antibacterial permanent antistatic composite material for foamed shoe materials comprises the following steps:

[0119] (1) Weigh the components in proportion for later use;

[0120] (2) Pour ethylene-vinyl acetate copolymer, graft-modified, polyaniline-modified halloysite nanotubes, and 4,4-oxydibenzenesulfonyl hydrazide into a stirring device according to weight parts and stir evenly to form material group A; pour polystyrene-polybutadiene-polystyrene triblock copolymer, nano-calcium carbonate, dicumyl peroxide, and an anti-aging agent into a stirring device according to weight parts and stir evenly to form material group B;

[0121] (3) Material group A is fed from the main feed of a twin-screw extruder, and material group B is fed from the side feed of the twin-screw extruder, and the mixture is melted, mixed, and extruded through the twin-screw extruder to obtain a polycarbonate composite material.

[0122] Among them, the set temperatures of the twin-screw extruder are: section one: 170°C, section two: 175°C, section three: 180°C, section four: 185°C, section five: 170°C, section six: 175°C, section seven: 175°C, section eight: 175°C, section nine: 180°C, and die head: 185°C.

[0123] Wherein, the rotation speed of the twin-screw extruder is 230rmp.

[0124] Comparative Example 1

[0125] Comparative Example 1 is substantially the same as Example 3, except that polyaniline-modified halloysite nanotubes are not added in Comparative Example 1.

[0126] Comparative Example 2

[0127] Comparative Example 2 is substantially the same as Example 3, except that no grafted modified nanosilver particles are added in Comparative Example 2.

[0128] Comparative Example 3

[0129] Comparative Example 3 is substantially the same as Example 3, except that nanosilver particles are added in Comparative Example 3.

[0130] The composite materials prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, and the specific tests were as follows: (1) density was measured according to ISO845-1988 standard;

[0131] (2) The rebound rate is tested according to GB / T1681 method;

[0132] (3) Surface resistance: Use a resistance meter to measure the resistance of the sample surface;

[0133] (4) Antibacterial test: Antibacterial test is carried out according to the standard "QB / T 2881-2013".

[0134] The test results are recorded in Table 1.

[0135] Table 1

[0136]

[0137] It can be seen from the data in Table 1 that the EVA composite material prepared by the present invention has light weight, excellent rebound and antibacterial properties, and good antistatic properties; and can be used as a shoe material in a clean environment.

[0138] From the data of Comparative Example 1, it can be seen that the effect of aniline-modified halloysite nanotubes on surface resistance is more obvious; the antibacterial property of the grafted modified nanosilver particles is equal to that of the pure nanosilver particles, indicating that the modification of the nanosilver particles in the present application does not reduce their antibacterial properties. In Comparative Example 2, which does not add nanosilver particles and grafted modified nanosilver particles, it can be seen that the grafted modified nanosilver particles and the nanosilver particles can effectively play the role of antibacterial agents.

[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An antibacterial permanent antistatic composite material for foaming shoe materials, characterized in that: In parts by weight, it comprises the following raw materials: 50-70 parts of ethylene-vinyl acetate copolymer, 10-20 parts of polystyrene-polybutadiene-polystyrene triblock copolymer, 10-20 parts of nano calcium carbonate, 3-6 parts of polyaniline modified halloysite nanotubes, 2-3 parts of 4,4-oxydibenzenesulfonyl hydrazide, Graft modified nano silver particles 1-2 parts, 0.7-1.2 parts of dicumyl peroxide, Anti-aging agent 0.4 to 1 part.

2. The antibacterial permanent antistatic composite material for foaming shoe materials according to claim 1, characterized in that: In parts by weight, it comprises the following raw materials: 55-65 parts of ethylene-vinyl acetate copolymer, 13-16 parts of polystyrene-polybutadiene-polystyrene triblock copolymer, 12-17 parts of nano calcium carbonate, 4-5 parts of polyaniline modified halloysite nanotubes, 2 to 2.5 parts of 4,4-oxydibenzenesulfonyl hydrazide, Graft modified nano silver particles 1.5-2 parts, 0.9-1.1 parts of dicumyl peroxide, Anti-aging agent 0.6-0.8 parts.

3. The antibacterial permanent antistatic composite material for foaming shoe materials according to any one of claims 1 to 2, characterized in that: In parts by weight, it is composed of the following raw materials: 55-65 parts of ethylene-vinyl acetate copolymer, 13-16 parts of polystyrene-polybutadiene-polystyrene triblock copolymer, 12-17 parts of nano calcium carbonate, 4-5 parts of polyaniline modified halloysite nanotubes, 2 to 2.5 parts of 4,4-oxydibenzenesulfonyl hydrazide, Graft modified nano silver particles 1.5-2 parts, 0.9-1.1 parts of dicumyl peroxide, Anti-aging agent 0.6-0.8 parts.

4. The antibacterial permanent antistatic composite material for foaming shoe materials according to claim 3, characterized in that: The particle size of the nano calcium carbonate is 400-500nm.

5. The antibacterial permanent antistatic composite material for foaming shoe materials according to claim 3, characterized in that: The anti-aging agent is selected from ethoxyquinoline or N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine.

6. The antibacterial permanent antistatic composite material for foaming shoe materials according to claim 3, characterized in that: The preparation method of the polyaniline modified halloysite nanotubes is: (1) Add 100 parts of water to a reaction container, then add 1.5 to 3.5 parts of dodecyldimethylsulfonyl betaine, turn on the stirring device to mix evenly; turn on the heater to raise the solution temperature to 50 to 60° C., then add 20 to 30 parts of halloysite nanotubes, and continue stirring for 10 to 20 minutes; (2) Add dilute hydrochloric acid to the reactor, stop adding when the pH reaches 4.6 to 4.7, and place the reactor in an ice bath at -5 to 0°C to wait for the solution temperature to stabilize; (3) adding 5 to 10 parts of aniline monomer to the reactor, controlling the stirring rate to 10 to 15 rpm, and applying ultrasound during the stirring process; then dripping 3 to 5 parts of ammonium persulfate solution into the reactor, wherein the dripping time is controlled to be 20 to 30 minutes; (4) The reaction solution of step (3) is filtered and washed with anhydrous ethanol and deionized water for 2 to 3 times, and the solid component is placed in a drying oven for drying to obtain polyaniline-modified halloysite nanotubes.

7. The antibacterial permanent antistatic composite material for foaming shoe materials according to claim 3, characterized in that: The preparation steps of the grafted modified nano silver particles are as follows: (1) tetrahydrofuran and water are mixed in a reactor at a volume ratio of 1:2 to form a 1L solution, 20-30g of silver particles with a particle size of 200nm are added thereto, and an inert gas is injected into the reactor; 0.5-1g of 2-butyl-6-phenylpyridine is added and stirred continuously; (2) Raise the temperature of the reactor to 50-60° C., add 0.1-0.2 g of azobisisobutyronitrile and react for 5-7 hours; (3) After the reaction is completed, the temperature is lowered to room temperature, the inert gas is stopped, and the stirring is stopped; the reaction solution is filtered, washed with anhydrous ethanol and deionized water in sequence; and dried to obtain the grafted modified nanosilver particles.

8. A method for preparing the antibacterial permanent antistatic composite material for foaming shoe materials as claimed in any one of claims 1 to 7, comprising the following steps: (1) Weigh the components in proportion for later use; (2) Pour ethylene-vinyl acetate copolymer, graft-modified, polyaniline-modified halloysite nanotubes, and 4,4-oxydibenzenesulfonyl hydrazide into a stirring device according to weight parts and stir evenly to form material group A; pour polystyrene-polybutadiene-polystyrene triblock copolymer, nano-calcium carbonate, dicumyl peroxide, and an anti-aging agent into a stirring device according to weight parts and stir evenly to form material group B; (3) Material group A is fed from the main feed of a twin-screw extruder, and material group B is fed from the side feed of the twin-screw extruder, and the mixture is melted, mixed, and extruded through the twin-screw extruder to obtain a polycarbonate composite material.

9. The method for preparing the antibacterial permanent antistatic composite material for foamed shoe materials according to claim 8, characterized in that: The twin-screw extruder has the following set temperatures: first stage: 165-175°C, second stage: 170-180°C, third stage: 175-185°C, fourth stage: 180-190°C, fifth stage: 165-175°C, sixth stage: 170~180℃, 7th stage: 170~180℃, 8th stage: 170~180℃, 9th stage: 175~185℃, machine head: 180~190℃.

10. The method for preparing the antibacterial permanent antistatic composite material for foamed shoe materials according to claim 8, characterized in that: The rotation speed of the twin-screw extruder is 200-250 rpm.

Citation Information

Cited By

  • Low-temperature-resistant and impact-resistant polypropylene foamed sheet and formula thereof

    CN121851548A