Environment-friendly plastic film material for preparing firework shell and preparation method of environment-friendly plastic film material
By using bio-based plastic powder and oyster shell powder, environmentally friendly plastic film materials are prepared, which solves the heat resistance, tear resistance and environmental protection of firework shell materials, and achieves efficient degradation and resources of materials Recycling improves production efficiency and product quality.
Patent Information
- Application Number
- CN202411065765.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
AI Technical Summary
The existing plastic film materials used in firework shells have shortcomings in terms of heat resistance, tear resistance and environmental protection, and their production and recycling problems are quite difficult, which violates the concept of green environmental protection.
Use bio-based plastic powder, oyster shell powder and chitin to prepare environmentally friendly plastic film materials through specific process treatment and formula design, including oyster shell pretreatment, calcination, crushing, grinding and other steps, combined with bio-based plastics Powder, polylactic acid, plasticizer and softener are used to prepare plastic films by blowing film.
It realizes the biodegradability of the materials, resource recycling, low toxicity and harmlessness, and good processing properties, has high strength, toughness and weather resistance, reduces environmental pollution and resource consumption, and meets the requirements of sustainable development.
Smart Images

Figure CN118931022A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new materials, and specifically discloses an environmentally friendly plastic film material for preparing a firework shell and a preparation method thereof. Background Art
[0002] Although the application of plastic film materials in the field of preparing fireworks shells is not as popular as in the fields of packaging, construction, agriculture, etc., it has also been used to a certain extent. Such materials are usually thin, transparent, and flexible, which allows fireworks to present a more gorgeous effect when displayed. However, in terms of the current development status, there are still some challenges and environmental deficiencies in the preparation of plastic film materials for fireworks shells. At present, the plastic film materials used for fireworks shells mainly include common plastics such as polyethylene (PE) and polypropylene (PP). These materials are selected for their good processing properties and cost-effectiveness. However, they also face the test of heat resistance, tear resistance and other properties, because fireworks will generate high temperatures and impact during the burning process. And the above materials have great deficiencies in environmental protection 1. Difficulty in degradation: Traditional plastic film materials are mostly made of petrochemical raw materials and are difficult to degrade in the natural environment. When fireworks are set off, their shells often become waste, causing long-term pollution to the environment. This is contrary to the current global advocacy of green environmental protection. 2. Resource consumption: The production of plastic film materials consumes a large amount of resources such as oil, which not only exacerbates the shortage of resources, but also may have a negative impact on the ecological environment. 3. Recycling and treatment problems: Due to the special properties of plastic film materials, it is difficult to recycle and treat them. At present, there is no complete recycling system and technical means to effectively treat the discarded plastic film materials of fireworks shells. Summary of the invention
[0003] In order to solve the above problems, the present invention discloses an environmentally friendly plastic film material for preparing firework shells and a preparation method thereof; the overall formula is intended to reduce environmental pollution and promote resource recycling, and is an ideal choice for preparing firework shells, showing the application prospects of green chemistry.
[0004] The technical solution of the present invention is as follows:
[0005] An environmentally friendly plastic film material for preparing a fireworks shell is made of the following raw materials in parts by weight:
[0006]
[0007]
[0008] Furthermore, in the above-mentioned environmentally friendly plastic film material for preparing fireworks shells, the oyster shell powder is prepared by the following process:
[0009] S1 Oyster shell pretreatment: first take the oyster shell, wash the surface with water, place it in a solution containing an oxidant for disinfection, and then oscillate it with ultrasound for 10-20 minutes with an ultrasonic power of 400-1000W. Then immerse the oyster shell in an acidic solution and heat it to 60-90℃ for 1-2 hours, pick it up, wash it, and dry it;
[0010] The oxidant is selected from one of potassium dichromate, sodium hypochlorite or hydrogen peroxide; the acidic solution is one of dilute hydrochloric acid, dilute sulfuric acid and dilute nitric acid;
[0011] S2 Calcination: The pretreated oyster shells are placed in a rotary kiln and heated to 180-220°C for calcination for 4-8 hours, and then cooled to room temperature;
[0012] S3 crushing: the calcined oyster shells are transferred to a crusher for primary crushing, and the oyster shells are sieved through a 300-mesh to 500-mesh sieve to obtain coarse oyster shell powder;
[0013] S4 grinding: transferring the crushed oyster shell powder to a powerful bead mill, adding an organic oligomer dispersant and a powder surface modifier, and grinding to ultrafine oyster shell powder with a particle size of 100-800 nm;
[0014] The organic oligomer dispersant is ethylene-vinyl acetate copolymer, and its addition amount is 0.5-1% of the mass of the oyster shell coarse powder;
[0015] The powder surface modifier is composed of the following raw materials in parts by mass:
[0016] 100 parts of magnesia and 10-20 parts of dioctyl phthalate; the added amount of the powder surface modifier is 1% of the mass of the oyster shell coarse powder.
[0017] Furthermore, in the above-mentioned environmentally friendly plastic film material for preparing firework shells, the plasticizer is epoxidized soybean oil, and the softener is pentaerythritol fatty acid ester.
[0018] Furthermore, in the above-mentioned environmentally friendly plastic film material for preparing a firework shell, the bio-based plastic powder is made of the following raw materials, calculated by weight:
[0019]
[0020]
[0021] Furthermore, in the above-mentioned environmentally friendly plastic film material for preparing firework shells, the plasticizer is glycerin and the lubricant is stearic acid.
[0022] Furthermore, in the above-mentioned environmentally friendly plastic film material for preparing a firework shell, the bio-based plastic powder is prepared by the following steps:
[0023] 1) After uniformly mixing linear low-density polyethylene, corn starch, straw powder, plasticizer, lubricant and maleic anhydride grafted PE, the mixture is put into a vacuum stirring kettle for reaction, the reaction temperature is controlled at 150-200° C., the vacuum degree is between 100-500 Pa, the stirring speed is 150-300 rpm, and the reaction time is 3-8 hours;
[0024] 2) After the reaction is completed, the material is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 150-180°C;
[0025] 3) After cooling, the granules are ground into powder and passed through a 100-200 mesh sieve to obtain bio-based plastic powder.
[0026] Furthermore, the present invention also discloses a method for preparing the above-mentioned environmentally friendly plastic film material for preparing a firework shell, comprising the following steps:
[0027] 1) In a reactor, the bio-based plastic powder and polylactic acid are first added according to the ratio, preliminarily mixed, and heated to 180-220° C., the pressure is controlled at 2-4 atmospheres, and the reaction is carried out for 2-4 hours;
[0028] 2) Then, cool down to 80-90°C, gradually add plasticizer and softener under normal pressure, and continue to stir and mix to ensure that all components are fully integrated;
[0029] 3) Maintaining the temperature at 80-90° C., add oyster shell powder and chitosan, and continue stirring and mixing until the oyster shell powder and chitosan are evenly distributed in the mixture without lumps;
[0030] 4) The material of step 3) is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 150-180°C.
[0031] Furthermore, the present invention also discloses the use of the above-mentioned environmentally friendly plastic film material in preparing a plastic film, and the environmentally friendly plastic film material is prepared into a plastic film using a film blowing method, comprising the following steps:
[0032] a. First, the block plastic film material is dried and crushed through a 300-500 mesh sieve to obtain a granular material;
[0033] b. Feed the granular material into the hopper of the film blowing machine, and heat and melt it into melt mixing and other pretreatment work, the melting temperature is 200-250℃, and then extrude the melt into a tubular structure;
[0034] c. Inject high-pressure air into the tubular structure to expand and stretch it into a thin film. By adjusting the pressure and speed of the airflow, the thickness and uniformity of the film can be controlled.
[0035] d. The film after blow molding needs to be quickly cooled and shaped by a cold air ring or other cooling device;
[0036] eFinally, the cooled film is rolled up using a winding device for subsequent processing and use.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The present invention discloses an environmentally friendly plastic film material for preparing a fireworks shell and a preparation method thereof, which has the following advancements compared to the prior art: 1. Biodegradability: The main components of the environmentally friendly plastic film material include bio-based plastic powder, polylactic acid, etc., and these raw materials have good biodegradability. After use, it can be decomposed by microorganisms in the natural environment, reducing long-term pollution to the environment and meeting the requirements of sustainable development. 2. Resource recycling: The utilization of oyster shell powder and straw powder realizes the resource recycling of waste and reduces the environmental pressure caused by landfill and incineration. At the same time, the application of corn starch as a renewable resource also promotes the effective utilization of agricultural resources. 3. Low toxicity and harmlessness: The plasticizer (such as epoxy soybean oil) and softener (such as pentaerythritol fatty acid ester) used are non-toxic or low-toxic substances, which are safer and more environmentally friendly than some harmful additives in traditional plastics, and are harmless to the human body and the environment. 4. Clean production process: The oxidant, acid solution, etc. used in the preparation process can be removed by cleaning and drying in the subsequent steps to ensure the purity of the final product, while also reducing the emission of wastewater and waste gas in the production process. 5 Through reasonable proportioning and process control, the environmentally friendly plastic film material has high strength and toughness while ensuring good degradability. The addition of oyster shell powder enhances the hardness and wear resistance of the material, while the addition of softener improves its flexibility and impact resistance. 6 Good processing performance: The material has good fluidity in the molten state, is easy to extrude and form, and the surface of the film produced is smooth and uniform in thickness. This is conducive to the subsequent film blowing process, improving production efficiency and product quality. 7 The specially treated oyster shell powder and chitin give the material better weather resistance and chemical stability, and can resist the influence of factors such as ultraviolet radiation and temperature changes within a certain range, extending the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is the tensile strength / Mpa test of the sample;
[0040] Figure 2 It is the elongation at break of the sample (%) test;
[0041] Figure 3 is the change rate of tensile strength of the sample under ultraviolet irradiation (%) (the smaller the better);
[0042] Figure 4 It is the change rate of tensile strength of the sample under hot air aging conditions (the smaller the better). DETAILED DESCRIPTION
[0043] An environmentally friendly plastic film material for preparing a fireworks shell is made of the following raw materials in parts by weight:
[0044]
[0045]
[0046] The oyster shell powder is prepared by the following process:
[0047] S1 Oyster shell pretreatment: first take the oyster shell, wash the surface with water, place it in a solution containing an oxidant for disinfection, and then oscillate it with ultrasound for 10-20 minutes with an ultrasonic power of 400-1000W. Then immerse the oyster shell in an acidic solution and heat it to 60-90℃ for 1-2 hours, pick it up, wash it, and dry it;
[0048] The oxidant is sodium hypochlorite; the acidic solution is dilute hydrochloric acid;
[0049] S2 Calcination: The pretreated oyster shells are placed in a rotary kiln and heated to 180-220°C for calcination for 4-8 hours, and then cooled to room temperature;
[0050] S3 crushing: the calcined oyster shells are transferred to a crusher for primary crushing, and the oyster shells are sieved through a 300-mesh to 500-mesh sieve to obtain coarse oyster shell powder;
[0051] S4 grinding: transferring the crushed oyster shell powder to a powerful bead mill, adding an organic oligomer dispersant and a powder surface modifier, and grinding to ultrafine oyster shell powder with a particle size of 100-800 nm;
[0052] The organic oligomer dispersant is ethylene-vinyl acetate copolymer, and its addition amount is 0.5-1% of the mass of the oyster shell coarse powder;
[0053] The powder surface modifier is composed of the following raw materials in parts by mass:
[0054] 100 parts of magnesia and 10-20 parts of dioctyl phthalate; the added amount of the powder surface modifier is 1% of the mass of the oyster shell coarse powder.
[0055] The bio-based plastic powder is made of the following raw materials, calculated by weight:
[0056]
[0057] The bio-based plastic powder is prepared by the following steps:
[0058] 1) After linear low-density polyethylene, corn starch, straw powder, glycerol, stearic acid and maleic anhydride grafted PE are mixed evenly, put into a vacuum stirring kettle for reaction, control the reaction temperature to 150-200° C., the vacuum degree to 100-500 Pa, the stirring speed to 150-300 rpm, and react for 3-8 hours;
[0059] 2) After the reaction is completed, the material is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 150-180°C;
[0060] 3) After cooling, the granules are ground into powder and passed through a 100-200 mesh sieve to obtain bio-based plastic powder.
[0061] The method for preparing the environmentally friendly plastic film material for preparing the shell of fireworks comprises the following steps:
[0062] 1) In a reactor, the bio-based plastic powder and polylactic acid are first added according to the ratio, preliminarily mixed, and heated to 180-220° C., the pressure is controlled at 2-4 atmospheres, and the reaction is carried out for 2-4 hours;
[0063] 2) Then, the temperature is lowered to 80-90° C., and under normal pressure, epoxy soybean oil and pentaerythritol fatty acid ester are gradually added, and stirring and mixing are continued to ensure that the components are fully integrated;
[0064] 3) Maintaining the temperature at 80-90° C., add oyster shell powder and chitosan, and continue stirring and mixing until the oyster shell powder and chitosan are evenly distributed in the mixture without lumps;
[0065] 4) Extrusion granulation: The material of step 3) is loaded into a twin-screw extruder for extrusion granulation, and the head temperature of the twin-screw extruder is 150-180°C.
[0066] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0067] Linear low-density polyethylene was purchased from Dongguan Meida Plastic Raw Materials Co., Ltd., brand LL 22B02.
[0068] Ethylene-vinyl acetate copolymer was purchased from Exxon EVA UL15028CC.
[0069] Maleic anhydride grafted PE was purchased from Mitsui Chemicals ADMER TM NF498E.
[0070] Polylactic acid was purchased from Hubei Jiufenglong Chemical Co., Ltd. and was dextrorotatory polylactic acid (PDLA) CAS 106989-11-1.
[0071] Example 1
[0072] An environmentally friendly plastic film material for preparing a fireworks shell is made of the following raw materials in parts by weight:
[0073]
[0074]
[0075] The oyster shell powder is prepared by the following process:
[0076] S1 Oyster shell pretreatment: First, take the oyster shell, wash the surface with water, and then place it in a solution containing an oxidant for disinfection, supplemented by ultrasonic vibration for 10 minutes, with an ultrasonic power of 1000W, then immerse the oyster shell in an acidic solution and heat it to 60°C, keep it for 1 hour, pick it up, wash it, and dry it;
[0077] The oxidant is sodium hypochlorite; the acidic solution is dilute hydrochloric acid;
[0078] S2 Calcination: The pretreated oyster shells are placed in a rotary kiln and heated to 180°C for calcination for 8 hours, and then cooled to room temperature;
[0079] S3 crushing: the calcined oyster shells are transferred to a crusher for primary crushing, and the oyster shells are sieved through a 300-mesh to 500-mesh sieve to obtain coarse oyster shell powder;
[0080] S4 grinding: transferring the crushed oyster shell powder to a powerful bead mill, adding an organic oligomer dispersant and a powder surface modifier, and grinding to ultrafine oyster shell powder with a particle size of 100-800 nm;
[0081] The organic oligomer dispersant is ethylene-vinyl acetate copolymer, and its addition amount is 0.5% of the mass of the oyster shell coarse powder;
[0082] The powder surface modifier is composed of the following raw materials in parts by mass:
[0083] 100 parts of magnesia and 10 parts of dioctyl phthalate; the added amount of the powder surface modifier is 1% of the mass of the oyster shell coarse powder.
[0084] The bio-based plastic powder is made of the following raw materials, calculated by weight:
[0085]
[0086] The bio-based plastic powder is prepared by the following steps:
[0087] 1) After linear low-density polyethylene, corn starch, straw powder, glycerol, stearic acid and maleic anhydride grafted PE are mixed evenly, put into a vacuum stirring kettle for reaction, and the reaction temperature is controlled at 150° C., the vacuum degree is between 100-500 Pa, the stirring speed is 150-300 rpm, and the reaction is carried out for 8 hours;
[0088] 2) After the reaction is completed, the material is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 150° C.;
[0089] 3) After cooling, the granules are ground into powder and passed through a 100-200 mesh sieve to obtain bio-based plastic powder.
[0090] The method for preparing the environmentally friendly plastic film material for preparing the shell of fireworks comprises the following steps:
[0091] 1) In a reactor, the bio-based plastic powder and polylactic acid are first added according to the ratio, preliminarily mixed, and heated to 180° C. The pressure is controlled at 2-4 atmospheres and the reaction is carried out for 4 hours;
[0092] 2) Then, the temperature is lowered to 80° C., and under normal pressure, epoxy soybean oil and pentaerythritol fatty acid ester are gradually added, and stirring and mixing are continued to ensure that the components are fully integrated;
[0093] 3) Maintaining the temperature at 80° C., add oyster shell powder and chitosan, and continue stirring and mixing until the oyster shell powder and chitosan are evenly distributed in the mixture without agglomeration;
[0094] 4) Extrusion granulation: The material of step 3) is loaded into a twin-screw extruder for extrusion granulation, and the head temperature of the twin-screw extruder is 150°C.
[0095] Example 2
[0096] An environmentally friendly plastic film material for preparing a fireworks shell is made of the following raw materials in parts by weight:
[0097]
[0098] The oyster shell powder is prepared by the following process:
[0099] S1 Oyster shell pretreatment: First, take the oyster shell, wash the surface with water, and then place it in a solution containing an oxidant for disinfection, supplemented by ultrasonic vibration for 15 minutes, with an ultrasonic power of 600W, then immerse the oyster shell in an acidic solution and heat it to 75°C, keep it for 1.5 hours, pick it up, wash it, and dry it;
[0100] The oxidant is sodium hypochlorite; the acidic solution is dilute hydrochloric acid;
[0101] S2 Calcination: The pretreated oyster shells are placed in a rotary kiln and heated to 200°C for calcination for 6 hours, and then cooled to room temperature;
[0102] S3 crushing: the calcined oyster shells are transferred to a crusher for primary crushing, and the oyster shells are sieved through a 300-mesh to 500-mesh sieve to obtain coarse oyster shell powder;
[0103] S4 grinding: transferring the crushed oyster shell powder to a powerful bead mill, adding an organic oligomer dispersant and a powder surface modifier, and grinding to ultrafine oyster shell powder with a particle size of 100-800 nm;
[0104] The organic oligomer dispersant is ethylene-vinyl acetate copolymer, and its addition amount is 0.75% of the mass of the oyster shell coarse powder;
[0105] The powder surface modifier is composed of the following raw materials in parts by mass:
[0106] 100 parts of magnesia and 15 parts of dioctyl phthalate; the added amount of the powder surface modifier is 1% of the mass of the oyster shell coarse powder.
[0107] The bio-based plastic powder is made of the following raw materials, calculated by weight:
[0108]
[0109] The bio-based plastic powder is prepared by the following steps:
[0110] 1) After linear low-density polyethylene, corn starch, straw powder, glycerol, stearic acid and maleic anhydride grafted PE are mixed evenly, put into a vacuum stirring kettle for reaction, and the reaction temperature is controlled at 180° C., the vacuum degree is between 100-500 Pa, the stirring speed is 150-300 rpm, and the reaction is carried out for 5 hours;
[0111] 2) After the reaction is completed, the material is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 170° C.;
[0112] 3) After cooling, the granules are ground into powder and passed through a 100-200 mesh sieve to obtain bio-based plastic powder.
[0113] The method for preparing the environmentally friendly plastic film material for preparing the shell of fireworks comprises the following steps:
[0114] 1) In a reactor, the bio-based plastic powder and polylactic acid are first added according to a ratio, preliminarily mixed, and heated to 200° C. The pressure is controlled at 2-4 atmospheres and the reaction is carried out for 3 hours;
[0115] 2) Then, the temperature is lowered to 85° C., and under normal pressure, epoxy soybean oil and pentaerythritol fatty acid ester are gradually added, and stirring and mixing are continued to ensure that the components are fully integrated;
[0116] 3) Maintaining the temperature at 85° C., add oyster shell powder and chitosan, and continue stirring and mixing until the oyster shell powder and chitosan are evenly distributed in the mixture without agglomeration;
[0117] 4) Extrusion granulation: The material of step 3) is loaded into a twin-screw extruder for extrusion granulation, and the head temperature of the twin-screw extruder is 165°C.
[0118] Example 3
[0119] An environmentally friendly plastic film material for preparing a fireworks shell is made of the following raw materials in parts by weight:
[0120]
[0121] The oyster shell powder is prepared by the following process:
[0122] S1 Oyster shell pretreatment: First, take the oyster shell, wash the surface with water, and then place it in a solution containing an oxidant for disinfection, supplemented with ultrasonic vibration for 20 minutes, with an ultrasonic power of 1000W, then immerse the oyster shell in an acidic solution and heat it to 90°C for 2 hours, pick it up, wash it, and dry it;
[0123] The oxidant is sodium hypochlorite; the acidic solution is dilute hydrochloric acid;
[0124] S2 Calcination: The pretreated oyster shells are placed in a rotary kiln and heated to 220°C for calcination for 8 hours, and then cooled to room temperature;
[0125] S3 crushing: the calcined oyster shells are transferred to a crusher for primary crushing, and the oyster shells are sieved through a 300-mesh to 500-mesh sieve to obtain coarse oyster shell powder;
[0126] S4 grinding: transferring the crushed oyster shell powder to a powerful bead mill, adding an organic oligomer dispersant and a powder surface modifier, and grinding to ultrafine oyster shell powder with a particle size of 100-800 nm;
[0127] The organic oligomer dispersant is ethylene-vinyl acetate copolymer, and its addition amount is 1% of the mass of the oyster shell coarse powder;
[0128] The powder surface modifier is composed of the following raw materials in parts by mass:
[0129] 100 parts of magnesia and 10-20 parts of dioctyl phthalate; the added amount of the powder surface modifier is 1% of the mass of the oyster shell coarse powder.
[0130] The bio-based plastic powder is made of the following raw materials, calculated by weight:
[0131]
[0132] The bio-based plastic powder is prepared by the following steps:
[0133] 1) After linear low-density polyethylene, corn starch, straw powder, glycerol, stearic acid and maleic anhydride grafted PE are mixed evenly, put into a vacuum stirring kettle for reaction, control the reaction temperature to 200°C, the vacuum degree to 100-500Pa, the stirring speed to 150-300rpm, and react for 3h;
[0134] 2) After the reaction is completed, the material is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 180° C.;
[0135] 3) After cooling, the granules are ground into powder and passed through a 100-200 mesh sieve to obtain bio-based plastic powder.
[0136] The method for preparing the environmentally friendly plastic film material for preparing the shell of fireworks comprises the following steps:
[0137] 1) In a reactor, the bio-based plastic powder and polylactic acid are first added according to the ratio, preliminarily mixed, and heated to 220° C. The pressure is controlled at 2-4 atmospheres and the reaction is carried out for 4 hours;
[0138] 2) Then, the temperature is lowered to 90° C., and under normal pressure, epoxy soybean oil and pentaerythritol fatty acid ester are gradually added, and stirring and mixing are continued to ensure that the components are fully integrated;
[0139] 3) Maintaining the temperature at 90° C., add oyster shell powder and chitosan, and continue stirring and mixing until the oyster shell powder and chitosan are evenly distributed in the mixture without agglomeration;
[0140] 4) Extrusion granulation: The material of step 3) is loaded into a twin-screw extruder for extrusion granulation, and the head temperature of the twin-screw extruder is 180°C.
[0141] Comparative Example 1
[0142] An environmentally friendly plastic film material for preparing a fireworks shell is made of the following raw materials in parts by weight:
[0143]
[0144]
[0145] The oyster shell powder is prepared by the following process:
[0146] S1 Oyster shell pretreatment: First, take the oyster shell, wash the surface with water, and then place it in a solution containing an oxidant for disinfection, supplemented by ultrasonic vibration for 15 minutes, with an ultrasonic power of 600W, then immerse the oyster shell in an acidic solution and heat it to 75°C, keep it for 1.5 hours, pick it up, wash it, and dry it;
[0147] The oxidant is sodium hypochlorite; the acidic solution is dilute hydrochloric acid;
[0148] S2 Calcination: The pretreated oyster shells are placed in a rotary kiln and heated to 200°C for calcination for 6 hours, and then cooled to room temperature;
[0149] S3 crushing: the calcined oyster shells are transferred to a crusher for primary crushing, and the oyster shells are sieved through a 300-mesh to 500-mesh sieve to obtain coarse oyster shell powder;
[0150] S4 grinding: transferring the crushed oyster shell powder to a powerful bead mill, adding an organic oligomer dispersant and a powder surface modifier, and grinding to ultrafine oyster shell powder with a particle size of 100-800 nm;
[0151] The organic oligomer dispersant is ethylene-vinyl acetate copolymer, and its addition amount is 0.75% of the mass of the oyster shell coarse powder;
[0152] The powder surface modifier is composed of the following raw materials in parts by mass:
[0153] 100 parts of magnesia and 15 parts of dioctyl phthalate; the added amount of the powder surface modifier is 1% of the mass of the oyster shell coarse powder.
[0154] The method for preparing the environmentally friendly plastic film material for preparing the shell of fireworks comprises the following steps:
[0155] 1) In a reactor, polyethylene and polylactic acid are first added according to the ratio, preliminarily mixed, and heated to 200°C, the pressure is controlled at 2-4 atmospheres, and the reaction is carried out for 3 hours;
[0156] 2) Then, the temperature is lowered to 85° C., and under normal pressure, epoxy soybean oil and pentaerythritol fatty acid ester are gradually added, and stirring and mixing are continued to ensure that the components are fully integrated;
[0157] 3) Maintaining the temperature at 85° C., add oyster shell powder and chitosan, and continue stirring and mixing until the oyster shell powder and chitosan are evenly distributed in the mixture without agglomeration;
[0158] 4) Extrusion granulation: The material of step 3) is loaded into a twin-screw extruder for extrusion granulation, and the head temperature of the twin-screw extruder is 165°C.
[0159] This comparative example uses polyethylene instead of bio-based plastic powder, and the rest is the same as Example 2.
[0160] Comparative Example 2
[0161] An environmentally friendly plastic film material for preparing a fireworks shell is made of the following raw materials in parts by weight:
[0162]
[0163] The bio-based plastic powder is made of the following raw materials, calculated by weight:
[0164]
[0165] The bio-based plastic powder is prepared by the following steps:
[0166] 1) After linear low-density polyethylene, corn starch, straw powder, glycerol, stearic acid and maleic anhydride grafted PE are mixed evenly, put into a vacuum stirring kettle for reaction, and the reaction temperature is controlled at 180° C., the vacuum degree is between 100-500 Pa, the stirring speed is 150-300 rpm, and the reaction is carried out for 5 hours;
[0167] 2) After the reaction is completed, the material is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 170° C.;
[0168] 3) After cooling, the granules are ground into powder and passed through a 100-200 mesh sieve to obtain bio-based plastic powder.
[0169] The method for preparing the environmentally friendly plastic film material for preparing the shell of fireworks comprises the following steps:
[0170] 1) In a reactor, the bio-based plastic powder and polylactic acid are first added according to a ratio, preliminarily mixed, and heated to 200° C. The pressure is controlled at 2-4 atmospheres and the reaction is carried out for 3 hours;
[0171] 2) Then, the temperature is lowered to 85° C., and under normal pressure, epoxy soybean oil and pentaerythritol fatty acid ester are gradually added, and stirring and mixing are continued to ensure that the components are fully integrated;
[0172] 3) Extrusion granulation: The material of step 2) is loaded into a twin-screw extruder for extrusion granulation, and the head temperature of the twin-screw extruder is 165°C.
[0173] Compared with Example 2, this comparative example does not contain oyster shell powder and chitosan.
[0174] Test Example 1
[0175] Strength and toughness test:
[0176] Experimental method: A universal material testing machine was used to conduct tensile tests and other mechanical property tests on the samples.
[0177] The sample is prepared by the following steps:
[0178] a. First, the block plastic film material is dried and crushed through a 300-500 mesh sieve to obtain a granular material;
[0179] b. Feed the granular material into the hopper of the film blowing machine, and heat and melt it into melt mixing and other pretreatment work, the melting temperature is 230℃, and then extrude the melt into a tubular structure;
[0180] c. Inject high-pressure air into the tubular structure to expand and stretch it into a thin film. By adjusting the pressure and speed of the airflow, the thickness and uniformity of the film can be controlled.
[0181] d. The film after blow molding needs to be quickly cooled and shaped by a cold air ring or other cooling device;
[0182] eFinally, the cooled film is rolled up using a winding device for subsequent processing and use.
[0183] The final prepared sample was 5x2cm and 0.1cm thick.
[0184] Evaluation indicators: mechanical performance parameters such as tensile strength and elongation at break; the results are shown in Table 1 and Figure 1 and Figure 2 .
[0185] Table 1 Strength and toughness test
[0186] Tensile strength / Mpa Elongation at break (%) Example 1 5.31 226 Example 2 5.36 221 Example 3 5.41 204 Comparative Example 1 4.37 184 Comparative Example 2 4.89 201
[0187] From the data in Table 1, it can be seen that the plastic film material prepared by using bio-based plastics containing linear low-density polyethylene to replace pure linear low-density polyethylene has better tensile strength and better toughness, while reducing the proportion of petrochemical polymers used, increasing the content of agricultural biowaste and degradable raw materials, and reducing environmental pressure.
[0188] Test Example 2
[0189] Prepare the sample using the method of Test Example 1.
[0190] UV irradiation aging test: According to GB / T16422.3-2014 "Plastics Laboratory Light Source Exposure Test Method Part 3: Fluorescent UV Lamp", the change rate of tensile strength of plastic film materials under the conditions of 55℃×18h and UV irradiation is tested.
[0191] Hot air aging test: According to GB / T7141-2008 "Plastics thermal aging test method", the change rate of tensile strength of plastic film materials under 105℃×240h conditions is tested.
[0192] The results are shown in Table 2 and Figure 3 and Figure 4 .
[0193] Table 2 UV and aging test
[0194]
[0195] From the data in Table 2 above, it can be seen that after adding oyster shell powder and chitosan to the formula, it can better resist ultraviolet light and hot air aging, and what is important is that the above raw materials are all natural products and are environmentally friendly.
[0196] It can be seen from the above embodiments and tests that the environmentally friendly plastic film material disclosed in the present invention is mainly composed of bio-based plastic powder, supplemented with degradable ingredients such as polylactic acid, and combined with plasticizers and softeners to improve processability and touch. The addition of oyster shell powder and chitosan not only enhances the strength and toughness of the material, but also enhances its anti-ultraviolet and anti-aging capabilities. The overall formula aims to reduce environmental pollution and promote resource recycling. It is an ideal choice for the preparation of firework shells and shows the application prospects of green chemistry.
[0197] The above are limited to several preferred embodiments of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. An environmentally friendly plastic film material for preparing fireworks shells, It is characterized in that Made from the following raw materials in parts by weight:
2. An environmentally friendly plastic film material for preparing a firework shell according to claim 1, It is characterized in that The oyster shell powder is prepared by the following process: S1 Oyster shell pretreatment: first take the oyster shell, wash the surface with water, place it in a solution containing an oxidant for disinfection, and then oscillate it with ultrasound for 10-20 minutes with an ultrasonic power of 400-1000W. Then immerse the oyster shell in an acidic solution and heat it to 60-90℃ for 1-2 hours, pick it up, wash it, and dry it; The oxidant is selected from one of potassium dichromate, sodium hypochlorite or hydrogen peroxide; the acidic solution is one of dilute hydrochloric acid, dilute sulfuric acid and dilute nitric acid; S2 Calcination: The pretreated oyster shells are placed in a rotary kiln and heated to 180-220°C for calcination for 4-8 hours, and then cooled to room temperature; S3 crushing: the calcined oyster shells are transferred to a crusher for primary crushing, and the oyster shells are sieved through a 300-mesh to 500-mesh sieve to obtain coarse oyster shell powder; S4 grinding: transferring the crushed oyster shell coarse powder to a powerful bead mill, adding an organic oligomer dispersant and a powder surface modifier, and grinding to ultrafine oyster shell powder with a particle size of 100-800 nm; The organic oligomer dispersant is ethylene-vinyl acetate copolymer, and its addition amount is 0.5-1% of the mass of the oyster shell coarse powder; The powder surface modifier is composed of the following raw materials in parts by mass: 100 parts of magnesia and 10-20 parts of dioctyl phthalate; the added amount of the powder surface modifier is 1% of the mass of the oyster shell coarse powder.
3. The environmentally friendly plastic film material for preparing a firework shell according to claim 1, It is characterized in that The plasticizer is epoxidized soybean oil, and the softener is pentaerythritol fatty acid ester.
4. The environmentally friendly plastic film material for preparing a firework shell according to claim 1, It is characterized in that The bio-based plastic powder is made of the following raw materials, calculated by weight:
5. An environmentally friendly plastic film material for preparing a firework shell according to claim 4, It is characterized in that The plasticizer is glycerol and the lubricant is stearic acid.
6. An environmentally friendly plastic film material for preparing a firework shell according to claim 4, It is characterized in that The bio-based plastic powder is prepared by the following steps: 1) After uniformly mixing linear low-density polyethylene, corn starch, straw powder, plasticizer, lubricant and maleic anhydride grafted PE, the mixture is put into a vacuum stirring kettle for reaction, the reaction temperature is controlled at 150-200° C., the vacuum degree is between 100-500 Pa, the stirring speed is 150-300 rpm, and the reaction time is 3-8 hours; 2) After the reaction is completed, the material is loaded into a twin-screw extruder for extrusion and granulation, and the head temperature of the twin-screw extruder is 150-180°C; 3) After cooling, the granules are ground into powder and passed through a 100-200 mesh sieve to obtain bio-based plastic powder.
7. A method for preparing an environmentally friendly plastic film material for preparing a fireworks shell according to any one of claims 1 to 6, It is characterized in that The following steps are involved: 1) In a reactor, the bio-based plastic powder and polylactic acid are first added according to the ratio, preliminarily mixed, and heated to 180-220° C., the pressure is controlled at 2-4 atmospheres, and the reaction is carried out for 2-4 hours; 2) Then, cool down to 80-90°C, gradually add plasticizer and softener under normal pressure, and continue to stir and mix to ensure that all components are fully integrated; 3) Maintaining the temperature at 80-90° C., add oyster shell powder and chitosan, and continue stirring and mixing until the oyster shell powder and chitosan are evenly distributed in the mixture without lumps; 4) Extrusion granulation: The material of step 3) is loaded into a twin-screw extruder for extrusion granulation, and the head temperature of the twin-screw extruder is 150-180°C.
8. Use of the environmentally friendly plastic film material according to any one of claims 1 to 6 in the preparation of plastic films, It is characterized in that The environmentally friendly plastic film material is prepared into a plastic film by using a film blowing method, comprising the following steps: a. First, the block plastic film material is dried and crushed through a 300-500 mesh sieve to obtain a granular material; b. Feed the granular material into the hopper of the film blowing machine, and heat and melt it into melt mixing and other pretreatment work, the melting temperature is 200-250℃, and then extrude the melt into a tubular structure; c. Inject high-pressure air into the tubular structure to expand and stretch it into a thin film. By adjusting the pressure and speed of the airflow, the thickness and uniformity of the film can be controlled. d. The film after blow molding needs to be quickly cooled and shaped by a cold air ring or other cooling device; eFinally, the cooled film is rolled up using a winding device for subsequent processing and use.