Super-oil-resistant and super-low-temperature-resistant polyolefin rubber material and preparation method thereof

By optimizing the formulation and preparation methods of polyolefin materials, the shortcomings of existing materials in oil resistance, low temperature resistance and mechanical properties are solved, and the requirements of EN50264 standard are met, and the costs are reduced and market competitiveness is enhanced.

CN118931028APending Publication Date: 2024-11-12ANHUI PACIFIC CABLE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411183624.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing irradiated crosslinked polyolefin materials are difficult to meet the strict requirements of the EN50264 standard for electrical performance, mechanical performance, aging resistance, oil resistance and low temperature resistance in the cable industry.

Method used

The preparation method of super oil resistant and super low temperature resistant polyolefin materials is adopted, including the optimized formula of components such as EVA700LX, EVA40LW, EVA421 ethylene-ethylene acetate copolymer, carbon black, TMQ, zinc stearate, zinc borate, aluminum hydroxide, etc. And through specific mixing, sulfur addition and filtration steps, the uniformity and performance of the material are improved.

Benefits of technology

It achieves excellent oil resistance, aging resistance, mechanical properties and low temperature resistance of the material, meets the requirements of the EN50264 standard, and reduces costs and improves market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931028A_ABST
    Figure CN118931028A_ABST
Patent Text Reader

Abstract

The invention discloses a polyolefin rubber material with super oil resistance and super low temperature resistance. The polyolefin rubber material is prepared from the following components in parts by weight: 30 to 40 parts of EVA 700LX rubber, 20 to 30 parts of EVA 40LW rubber, 10 to 20 parts of EVA 421 ethylene-vinyl acetate copolymer, 5 to 10 parts of reinforcing agent, 3 to 5 parts of anti-aging agent TMQ, 2 to 4 parts of vulcanizing agent 14S, 1 to 3 parts of accelerant, 1.5 to 3 parts of lubricant, 1 to 2 parts of softening agent (BN-18), 0.5 to 1.5 parts of DOS oil, 0.5 to 1 part of flame retardant, 1 to 2 parts of coupling agent (FD-172), 3 to 5 parts of branching agent P-250 and 150 to 200 parts of flame-retardant filler. The invention also relates to a preparation method of the super-oil-resistant super-low-temperature-resistant polyolefin rubber material. The preparation method comprises the following steps: S1, raw material pretreatment; s2, primary mastication; s3, feeding and mixing; s4, filtering rubber; s5, open milling; and S6, sulfur addition. By optimizing the formula, the prepared EVA rubber material has excellent oil resistance, aging resistance and mechanical properties, and can meet the requirements of the EN50264 standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an oil-resistant and low-temperature-resistant polyolefin material technology, and in particular to a super oil-resistant and super low-temperature-resistant polyolefin rubber and a preparation method thereof. Background Art

[0002] With the continuous development of electrical equipment and cable industry, the performance requirements for cable materials are getting higher and higher. EN50264 standard puts forward strict requirements on cable materials in terms of electrical performance, mechanical performance, aging resistance, oil resistance, low temperature resistance, etc. At present, the radiation cross-linked polyolefin materials on the market have deficiencies in some performance aspects and are difficult to fully meet the standard. Therefore, a super oil-resistant and super low temperature-resistant polyolefin rubber and its preparation method are proposed. Summary of the invention

[0003] The purpose of the present invention is to provide a super oil-resistant and super low-temperature-resistant polyolefin rubber and a preparation method thereof, so as to solve the performance deficiencies of existing radiation cross-linked polyolefin materials and the problems existing in production technology.

[0004] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:

[0005] The invention discloses a super oil-resistant and super low-temperature-resistant polyolefin rubber and a preparation method thereof. The polyolefin rubber comprises the following components by weight: 30-40 parts of EVA700LX rubber, 20-30 parts of EVA40LW rubber, 10-20 parts of EVA421 ethylene-vinyl acetate copolymer, 5-10 parts of reinforcing agent, 3-5 parts of antioxidant TMQ, 2-4 parts of vulcanizing agent 14S, 1-3 parts of accelerator, 1.5-3 parts of lubricant, 1-2 parts of softener (BN-18), 0.5-1.5 parts of DOS oil, 0.5-1 parts of flame retardant, 1-2 parts of coupling agent (FD-172), 3-5 parts of branching agent P-250 and 150-200 parts of flame retardant filler.

[0006] Furthermore, the reinforcing agent is carbon black N330, the accelerator is TAC powder, the lubricant is zinc stearate, the flame retardant is zinc borate, and the flame retardant filler is aluminum hydroxide.

[0007] A method for preparing a super oil-resistant and super low-temperature-resistant polyolefin rubber material comprises the following steps:

[0008] S1. Raw material pretreatment: Cut EVA700 rubber, EVA40LW rubber and EVA421 ethylene-vinyl acetate copolymer into small pieces to make subsequent mixing more uniform; at the same time, dry carbon black N330, TMQ and TAC powder to remove moisture and impurities to ensure the purity and quality of the raw materials;

[0009] S2, primary mastication: adding the pretreated EVA700LX rubber, EVA40LW rubber and EVA421 ethylene-vinyl acetate copolymer into an internal mixer for mixing; the temperature of the internal mixer is controlled at 100-120°C, the speed is set to a suitable value, and the mixing time is 10-15 minutes, so that the three rubbers are fully mixed;

[0010] S3, adding materials and mixing: after the first mixing is completed, gradually add reinforcing agent (carbon black) N330, antioxidant TMQ, lubricant (zinc stearate), softener (BN-18), DOS oil, flame retardant (zinc borate), flame retardant filler (aluminum hydroxide) into the internal mixer in sequence; after each addition, mix for 8-10 minutes to ensure that various additives are fully integrated with the rubber; during the whole adding process, the temperature of the internal mixer is maintained at 120-140°C;

[0011] S4, rubber filtering: Take out the mixed material and put it into the rubber filter to filter and remove impurities in the raw material. Use 40 mesh, 60 mesh and 80 mesh filter screens. Replace the screens when they are worn out. Keep the temperature of the rubber filter at 60-80℃.

[0012] S5, open refining; take out the mixed material, put it into the open mill for thin passing, the number of thin passing is 3-5 times, so that the thickness of the material is uniform, and further remove the bubbles and impurities that may exist therein; then roll the material down and park it for 12-24 hours to allow the various components inside the material to fully diffuse and react to reach a uniform and stable state;

[0013] S6. Vulcanization: Put the parked materials into an internal mixer for vulcanization; add vulcanizing agent 14S, accelerator (TAC powder), coupling agent (FD-172), and branching agent (P-250) in sequence, set the temperature of the internal mixer to 80-100°C, and the vulcanization time is 3-5 minutes; during the vulcanization process, strictly control the temperature and time to ensure that the vulcanizing agent in the rubber material is fully and evenly integrated.

[0014] The present invention has the following beneficial effects:

[0015] The invention optimizes the formula so that the prepared EVA rubber material has excellent oil resistance, aging resistance and mechanical properties and can meet the requirements of EN50264 standard; the synergistic effect of EVA700LX, EVA40LW and EVA421 ethylene-vinyl acetate copolymers effectively improves the oil resistance, low temperature resistance and aging resistance of the material; the addition of N330 and antioxidant TMQ enhances the mechanical properties of the material; the addition of zinc stearate and BN-18 improves the processing properties of the material; the use of DOS oil, flame retardant (zinc borate), coupling agent (FD-172) and branching agent P-250 further enhances the comprehensive properties of the material; and at the same time, through cost control measures, the product has high cost performance while having good performance, thereby enhancing market competitiveness.

[0016] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0018] Figure 1 The present invention is a flow chart of a method for preparing a super oil-resistant and super low-temperature-resistant polyolefin rubber material. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the description of the present invention, it should be understood that the terms "upper", "middle", "outer", "inner" and the like indicating directions or positional relationships are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the components or elements referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as limiting the present invention.

[0021] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0022] See also Figure 1 As shown, the super oil-resistant and super low-temperature resistant polyolefin rubber of this embodiment includes the following components, by mass: 30-40 parts of EVA700LX rubber, 20-30 parts of EVA40LW rubber, 10-20 parts of EVA421 ethylene-vinyl acetate copolymer, 5-10 parts of reinforcing agent, 3-5 parts of antioxidant TMQ, 2-4 parts of vulcanizing agent 14S, 1-3 parts of accelerator, 1.5-3 parts of lubricant, 1-2 parts of softener (BN-18), 0.5-1.5 parts of DOS oil, 0.5-1 parts of flame retardant, 1-2 parts of coupling agent (FD-172), 3-5 parts of branching agent P-250, and 150-200 parts of flame retardant filler.

[0023] Furthermore, the reinforcing agent is carbon black N330, the accelerator is TAC powder, the lubricant is zinc stearate, the flame retardant is zinc borate, and the flame retardant filler is aluminum hydroxide.

[0024] It should be further explained that polyolefin rubber has many significant performance advantages:

[0025] In terms of electrical performance, it exhibits extremely outstanding characteristics. It has extremely high insulation resistance, which can effectively block abnormal leakage of current and build a reliable protective barrier for power transmission. At the same time, it has excellent dielectric strength and can withstand large electric field strength without being broken down, ensuring the stability and safety of power transmission. The low dielectric loss factor ensures the accuracy and efficiency of the signal during transmission, greatly reducing energy loss and enabling electrical energy and signals to be transmitted accurately and efficiently.

[0026] In terms of mechanical properties, it has remarkable tensile strength, which enables it to withstand large tensile forces without breaking easily; the high elongation at break gives the rubber material excellent flexibility and ductility, and it can maintain good integrity when facing complex usage environments and variable external forces, such as stretching, bending, twisting, etc., and is not prone to rupture or damage; in addition, good wear resistance also allows the rubber material to maintain its own stable performance during long-term use, even if it frequently rubs and contacts with other objects, effectively extending the service life of cables and related products.

[0027] The aging resistance is very good. During long-term use, whether it is exposed to high temperature, high humidity environment, or exposed to ultraviolet rays, it can maintain stable performance; the added antioxidant can effectively resist the erosion of various aging factors such as oxidation, thermal aging and light aging, and significantly slow down the aging rate of the rubber material, so that it can still maintain good physical and chemical properties during long-term service, thereby extending the service life of the product and reducing maintenance and replacement costs.

[0028] The flame retardant performance is outstanding. The scientific addition of flame retardants enables the rubber material to quickly extinguish itself when encountering open flames, effectively preventing the spread of flames. This feature greatly reduces the risk of fire and provides higher safety guarantees for the places of use, especially in some environments with extremely strict fire protection requirements, such as high-rise buildings, power facilities, etc., its advantages are particularly obvious.

[0029] Excellent oil resistance, the ability to maintain stable physical and chemical properties when in contact with various oils (such as mineral oil, fuel oil, etc.). Specifically, the material does not swell, soften, become brittle, lose strength, deform, change color, or change weight too much when immersed, washed or in long-term contact with oil; indicators for measuring oil resistance include volume change rate, mass change rate, hardness change, tensile strength change, elongation at break change, etc.

[0030] Low temperature resistance means that the material can still maintain good physical properties and operability in a low temperature environment. The material will not become brittle, crack, harden or become brittle, leading to loss of elasticity or ductility, etc. at low temperatures. Generally, the low temperature resistance of the material is evaluated by measuring its low temperature brittleness temperature, cold bending performance, low temperature impact strength, etc. In a low temperature environment, the molecular movement of the material slows down, which may lead to a decrease in its mechanical properties. The material of the present invention has good low temperature resistance and can still maintain the necessary strength, toughness and flexibility at lower temperatures to meet work requirements.

[0031] The preparation method of the super oil-resistant and super low-temperature-resistant polyolefin rubber material of the present embodiment comprises the following steps:

[0032] S1. Raw material pretreatment: Cut EVA700 rubber, EVA40LW rubber and EVA421 ethylene-vinyl acetate copolymer into small pieces to make subsequent mixing more uniform; at the same time, dry carbon black N330, TMQ and TAC powder to remove moisture and impurities to ensure the purity and quality of the raw materials;

[0033] S2, primary mastication: adding the pretreated EVA700LX rubber, EVA40LW rubber and EVA421 ethylene-vinyl acetate copolymer into an internal mixer for mixing; the temperature of the internal mixer is controlled at 100-120°C, the speed is set to a suitable value, and the mixing time is 10-15 minutes, so that the three rubbers are fully mixed;

[0034] S3, adding materials and mixing: after the first mixing is completed, gradually add reinforcing agent (carbon black) N330, antioxidant TMQ, lubricant (zinc stearate), softener (BN-18), DOS oil, flame retardant (zinc borate), flame retardant filler (aluminum hydroxide) into the internal mixer in sequence; after each addition, mix for 8-10 minutes to ensure that various additives are fully integrated with the rubber; during the whole adding process, the temperature of the internal mixer is maintained at 120-140°C;

[0035] S4, rubber filtering: Take out the mixed material and put it into the rubber filter to filter and remove impurities in the raw material. Use 40 mesh, 60 mesh and 80 mesh filter screens. Replace the screens when they are worn out. Keep the temperature of the rubber filter at 60-80℃.

[0036] S5, open refining; take out the mixed material, put it into the open mill for thin passing, the number of thin passing is 3-5 times, so that the thickness of the material is uniform, and further remove the bubbles and impurities that may exist therein; then roll the material down and park it for 12-24 hours to allow the various components inside the material to fully diffuse and react to reach a uniform and stable state;

[0037] S6. Vulcanization: Put the parked materials into an internal mixer for vulcanization; add vulcanizing agent 14S, accelerator (TAC powder), coupling agent (FD-172), and branching agent (P-250) in sequence, set the temperature of the internal mixer to 80-100°C, and the vulcanization time is 3-5 minutes; during the vulcanization process, strictly control the temperature and time to ensure that the vulcanizing agent in the rubber material is fully and evenly integrated.

[0038] It should be further explained that the polyolefin rubber of the present invention has good electrical properties, mechanical properties, aging resistance, flame retardancy, oil resistance and low temperature resistance, and can fully meet the requirements of EN50264 standard. It has a wide range of applications and is suitable for the following scenarios:

[0039] Vehicle cables in the rail transit field provide reliable power and signal transmission guarantees for the stable operation of trains.

[0040] Control cables in the field of industrial automation ensure precise control of equipment and data transmission in complex industrial environments.

[0041] Cables used in ships and marine engineering can work stably for a long time in harsh environments such as humidity and salt spray.

[0042] The medium and low voltage cables in the power system of railway locomotives ensure the safe transmission of electricity in high-speed railway trains.

[0043] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0044] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A super oil-resistant and super low-temperature-resistant polyolefin rubber material, characterized in that: The polyolefin rubber material comprises the following components in parts by mass: 30-40 parts of EVA700LX rubber, 20-30 parts of EVA40LW rubber, 10-20 parts of EVA421 ethylene-vinyl acetate copolymer, 5-10 parts of reinforcing agent, 3-5 parts of antioxidant TMQ, 2-4 parts of vulcanizing agent 14S, 1-3 parts of accelerator, 1.5-3 parts of lubricant, 1-2 parts of softener (BN-18), 0.5-1.5 parts of DOS oil, 0.5-1 parts of flame retardant, 1-2 parts of coupling agent (FD-172), 3-5 parts of branching agent P-250, and 150-200 parts of flame retardant filler.

2. A super oil-resistant and super low-temperature-resistant polyolefin rubber material and a preparation method thereof according to claim 1, characterized in that: The reinforcing agent is carbon black N330, the accelerator is TAC powder, the lubricant is zinc stearate, the flame retardant is zinc borate, and the flame retardant filler is aluminum hydroxide.

3. The method for preparing a super oil-resistant and super low-temperature-resistant polyolefin rubber according to claim 1, characterized in that: The following steps are involved: S1. Raw material pretreatment: Cut EVA700 rubber, EVA40LW rubber and EVA421 ethylene-vinyl acetate copolymer into small pieces to make subsequent mixing more uniform; at the same time, dry carbon black N330, TMQ and TAC powder to remove moisture and impurities to ensure the purity and quality of the raw materials; S2, primary mastication: adding the pretreated EVA700LX rubber, EVA40LW rubber and EVA421 ethylene-vinyl acetate copolymer into an internal mixer for mixing; the temperature of the internal mixer is controlled at 100-120°C, the speed is set to a suitable value, and the mixing time is 10-15 minutes, so that the three rubbers are fully mixed; S3, adding materials and mixing: after the first mixing is completed, gradually add reinforcing agent (carbon black) N330, antioxidant TMQ, lubricant (zinc stearate), softener (BN-18), DOS oil, flame retardant (zinc borate), flame retardant filler (aluminum hydroxide) into the internal mixer in sequence; after each addition, mix for 8-10 minutes to ensure that various additives are fully integrated with the rubber; during the whole adding process, the temperature of the internal mixer is maintained at 120-140°C; S4, rubber filtering: Take out the mixed material and put it into the rubber filter to filter and remove impurities in the raw material. Use 40 mesh, 60 mesh and 80 mesh filter screens. Replace the screens when they are worn out. Keep the temperature of the rubber filter at 60-80℃. S5, open refining: take out the mixed material and put it into the open refining mill for thin passing 3-5 times to make the thickness of the material uniform and further remove the bubbles and impurities that may exist therein; then roll the material and leave it for 12-24 hours to allow the various components inside the material to fully diffuse and react to reach a uniform and stable state; S6. Vulcanization: Put the parked materials into an internal mixer for vulcanization; add vulcanizing agent 14S, accelerator (TAC powder), coupling agent (FD-172), and branching agent (P-250) in sequence, set the temperature of the internal mixer to 80-100°C, and the vulcanization time is 3-5 minutes; during the vulcanization process, strictly control the temperature and time to ensure that the vulcanizing agent in the rubber material is fully and evenly integrated.

Citation Information

Cited By

  • Mould-resistant halogen-free low-smoke flame-retardant rubber sheath material and preparation method thereof

    CN119735886A