Wear-resistant halogen-free low-smoke flame-retardant polyolefin cable material as well as preparation method and application thereof
By using polymer substrates, powdered carboxylic nitrile rubber and other materials and radiation grafting technology in cable materials, combined with electronic accelerator radiation crosslinking, wear-resistant, halogen-free, low smoke and flame-retardant polyolefin cable materials are prepared, which solves the high cost The problem of high processing temperature meets the low smoke, halogen-free and flame retardant requirements of rolling stock cables, and improves the oil resistance of cable materials.
Patent Information
- Application Number
- CN202411183741.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
The existing cable materials are due to high cost and high processing temperature, and it is difficult to meet the low smoke, halogen-free and flame-retardant requirements of rolling stock cables.
Using polymer substrates, powdered carboxylic nitrile rubber, inorganic flame retardant, polyphosphazene flame retardant, montmorillonite synergistic flame retardant, composite antioxidant and processing aid, maleic anhydride is grafted through radiation Ethylene-vinyl acetate copolymer and nylon 12 elastomer are combined with electronic accelerator radiation crosslinking to prepare wear-resistant, halogen-free, low smoke and flame-retardant polyolefin cable materials.
The cable material has achieved oil-resistant, wear-resistant, low smoke, halogen-free and flame-retardant properties, meets relevant standards and reduces costs and simplifies processing temperature.
Smart Images

Figure BDA0005012941720000051 
Figure BDA0005012941720000061 
Figure BDA0005012941720000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials, and in particular relates to a wear-resistant, halogen-free, low-smoke, flame-retardant polyolefin cable material and a preparation method and application thereof. Background Art
[0002] Cable materials are raw materials used to form insulation and sheath layers in the production process of wires and cables. There are many types of wires and cables, and different types of wires and cables have different performance requirements. Locomotive and vehicle cables (wires) are mainly used in high-speed railways and urban rail vehicles. According to regulations, cables (wires) for electrical devices in the power distribution system, control system, and signal system of locomotives and urban rail vehicles must meet the requirements of being suitable for narrow spaces, low smoke, halogen-free, and flame-retardant.
[0003] At present, many cable factories in China have been able to produce 125℃ oil-resistant halogen-free flame-retardant locomotive vehicle cables, and there are also many invention patents for radiation cross-linked oil-resistant halogen-free flame-retardant cable materials, such as patent CN103937086A (125℃ irradiation cross-linked oil-resistant low-smoke halogen-free flame-retardant cable materials and preparation methods thereof), the polymer uses ethylene-vinyl acetate copolymer (EVA) + nylon 12 elastomer (PA12 elastomer) + nylon 12 grafted maleic anhydride (PA12-g-MAH). The prepared cable material is wear-resistant and oil-resistant. Due to the high cost of PA12 elastomer, the price of the prepared cable material is relatively high, and the melting temperature of PA12 elastomer is 240-300℃, which increases the processing temperature and difficulty of cable materials and cables. Summary of the invention
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: the wear-resistant halogen-free low-smoke flame-retardant polyolefin cable material comprises, by weight, 100 parts of a polymer base material, 5-10 parts of powdered carboxyl nitrile rubber, 120-140 parts of an inorganic flame retardant, 5-15 parts of a polyphosphazene flame retardant, 3-6 parts of a montmorillonite synergistic flame retardant, 1.5-3 parts of a composite antioxidant, 5-8 parts of a processing aid, and 3-5 parts of an environmentally friendly masterbatch; the polymer base material comprises 3-5 parts of a radiation-grafted maleic acid Ethylene-vinyl acetate copolymer with maleic anhydride (EVA-g-MAH) and / or 3-5 parts of radiation grafted maleic anhydride nylon 12 elastomer (PA12-g-MAH), 30-50 parts of ethylene-vinyl acetate copolymer with low vinyl acetate ((VA=28%, MI=4-6)) content (EVA) and / or 40-60 parts of ethylene-vinyl acetate copolymer elastomer (EVM) with high vinyl acetate (VA=50%, MI=4-6) content.
[0005] As a preferred embodiment of the above technical solution, the inorganic flame retardant includes any one or more of silane-treated magnesium hydroxide and silane-treated aluminum hydroxide; the polyphosphazene flame retardant includes hexaphenoxy cyclotriphosphazene and phenoxy polyphosphazene; the composite antioxidant includes a main antioxidant and an auxiliary antioxidant, wherein the main antioxidant includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (1010), pentaerythritol tetrakis(3-laurylthiopropionate) (412S), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl (300), N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] The invention relates to a process for preparing the present invention, wherein the present invention comprises any one or more of: a thioester antioxidant, dioctadecyl thiopropionate (DLTP) and dioctadecyl thiopropionate (DSTP); the processing aid comprises a cross-linking sensitizer and a lubricant, wherein the cross-linking sensitizer comprises any one or more of trimethylolpropane trimethacrylate (TMPTMA) and triallyl isocyanurate (TAIC); and the lubricant comprises any one or more of polyethylene wax (PE wax), zinc stearate, ethylene bisstearamide (EBS) and silicone masterbatch.
[0006] As a preferred embodiment of the above technical scheme, the weight ratio of silane-treated magnesium hydroxide and silane-treated aluminum hydroxide in the inorganic flame retardant is 60-80:40-60; the weight ratio of hexaphenoxy cyclotriphosphazene and phenoxy polyphosphazene in the polyphosphazene flame retardant is 5-15:0-4; the weight ratio of the main antioxidant and the auxiliary antioxidant in the composite antioxidant is 1:1-3; the industrial auxiliary agent includes 1-2 parts of a cross-linking sensitizer and 3-5 parts of a lubricant.
[0007] As a preferred embodiment of the above technical solution, the average particle size of the montmorillonite synergistic flame retardant is 16-22 μm.
[0008] The preparation method of wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material comprises the following steps: weighing a polymer substrate, powdered carboxyl nitrile rubber (radiation-cured ultrafine nano-carboxyl nitrile rubber prepared by Beijing Institute of Chemical Technology, brand VP501, particle size 90nm), inorganic flame retardant, polyphosphazene flame retardant, montmorillonite synergistic flame retardant, composite antioxidant, processing aid and environmentally friendly masterbatch, mixing in an internal mixer, melt mixing to a temperature range of 140-160°C, then lifting to a two-stage twin-screw extruder, extruding and granulating by air cooling in a temperature range of 130-170°C, and obtaining the wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material.
[0009] As a preferred embodiment of the above technical solution, the radiation grafted maleic anhydride ethylene-vinyl acetate copolymer is prepared according to the following steps: 2-5 parts of maleic anhydride are dissolved in acetone, mixed with 100 parts of ethylene-vinyl acetate copolymer (VA=28%, MI=4-6) in a high-speed mixer, and after the acetone is completely volatilized, granulated in a twin-screw extruder at 100-130°C water ring, and then radiation grafted in an electron accelerator at 3-5Mev, with an irradiation dose of 10-25kGy, to obtain 1-3% grafting rate and ≤10% of ethylene-vinyl acetate radiation grafted maleic anhydride ethylene-vinyl acetate Ester copolymer; the radiation grafted maleic anhydride nylon 12 elastomer is prepared by the following method: 2-5 parts of maleic anhydride are dissolved in acetone, and mixed with 100 parts of nylon 12 elastomer (adopting French Arkema nylon elastomer Pebax series, Shore hardness 55D) in a high-speed mixer, and after the acetone is completely volatilized, granulation is carried out in a twin-screw extruder at 200-230°C water ring, and then radiation grafting is carried out in an electron accelerator at 3-5Mev, and the irradiation dose is 10-25kGy, to obtain a radiation grafted maleic anhydride nylon 12 elastomer with a grafting rate of 1-3% and a gel content of ≤10%.
[0010] The application of wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material is to extrude the wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material on the wire and cable extruder production line, control the temperature at 120-160°C, and coat the cable material on the conductor core; then radiate cross-linking in an electron accelerator with an energy of 1.5-5Mev, the irradiation dose is 100-150kGy, and the thermal extension is controlled at 20-40%.
[0011] The beneficial effects of the present invention are as follows: the wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material of the present invention improves the oil resistance of the cable material by adding powdered carboxyl nitrile rubber, and improves the wear resistance of the cable material by adding a nylon 12 elastomer compatibilizer of radiation grafted maleic anhydride. The cable material meets the standard requirements of halogen-free, low-smoke, flame-retardant insulation materials and sheath materials of GB / T12528-2008 and EN50264 standards, and has excellent flame retardant effect. The flame retardant grade of the prepared wire and cable passes the single vertical combustion test of finished cables of GB / T18380.1-2001 or GB / T18380.2-2001 standards, the cable bundle combustion test meets the requirements of GB / T18380.3-2001 standards, and the oil resistance passes the mineral oil and fuel oil immersion test in Supplement 1 of GB12528.11-2003. The temperature resistance grade is 125°C and has excellent wear resistance. DETAILED DESCRIPTION
[0012] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0013] Prepare the components of oil-resistant cable materials according to the formula in the table. Use a weight loss scale to transport the components through pipelines into an internal mixer for mixing, melt mixing to a temperature range of 140-160°C, and then promote to a two-stage twin-screw extruder, air-cooled extrusion granulation at a temperature range of 130-170°C to obtain cable materials. Control the temperature of part of the cable material on the wire and cable extruder production line at 120-160°C to extrude and coat the cable material on the conductor core. Radiation cross-link the wires and cables in an electron accelerator with an energy of 1.5-5Mev, an irradiation dose of 100-150kGy, and a thermal extension control of 20-40%.
[0014] Example 1
[0015]
[0016]
[0017] Example 2
[0018]
[0019] Example 3
[0020]
[0021]
[0022] Example 4
[0023]
[0024]
[0025] Example 5
[0026]
[0027]
[0028] Example 6
[0029]
[0030] The cable materials and irradiation cross-linked cables prepared in the above embodiments were subjected to performance tests, and the test results are shown in the following table:
[0031] Performance of irradiated cross-linked cable materials (irradiation dose 120KGy)
[0032]
[0033]
[0034]
[0035] Irradiation cross-linked cable performance (irradiation dose 120KGy)
[0036]
[0037]
[0038]
[0039]
[0040]
[0041]
[0042] By comparing the cable materials prepared in Examples 1-6 of the present invention and the performance of the cables prepared therefrom, the following results can be obtained:
[0043] (1) The formulations of Example 1 and Example 2 are the same except for the type of compatibilizer. Example 1 uses compatibilizer EVA-g-MAH, while Example 2 uses compatibilizers EVA-g-MAH and PA12-g-MAH. The oil resistance of Example 2 is obviously better than that of Example 1, and the wear resistance of Example 1 does not meet the requirements, indicating that the compatibilizer PA12-g-MAH has better oil resistance and wear resistance.
[0044] (2) The formula of Example 2 is the same as that of Example 3, except that Example 3 adds 10 kg of inorganic flame retardant and has the same other ingredients. The cable prepared in Example 3 passed the single vertical burning test of the cable, while Example 2 failed the single vertical burning test of the cable.
[0045] (3) The formula of Example 3 and Example 4, Example 4 adds more compatibilizer PA12-g-MAH, and the oil resistance is better, but other properties are slightly reduced, and the cost is higher and the processing temperature is also increased.
[0046] (4) The formula of Example 3 is different from that of Examples 5 and 6. Examples 5 and 6 increase the amount of powdered carboxyl nitrile rubber added, and the softness and oil resistance of the material and the cable are improved, but the tensile strength is reduced.
[0047] The wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable materials prepared in Examples 1-6 of the present invention and the properties of the cables prepared therefrom are as follows: 1. The compatibilizer PA12-g-MAH has excellent oil resistance and wear resistance; 2. The powdered carboxyl nitrile rubber has good oil resistance.
[0048] It is worth mentioning that the technical features of the internal mixer, wire and cable extruder production line, electron accelerator, etc. involved in the patent application of this invention should be regarded as the prior art. The specific structure, working principle and possible control method and spatial layout method of these technical features can be selected by conventional methods in the field, and should not be regarded as the inventive point of the patent of this invention. The patent of this invention will not be further elaborated.
[0049] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the existing technology should be within the scope of protection determined by the claims.
Claims
1. Wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material, characterized in that: The invention comprises, by weight, 100 parts of a polymer matrix, 5-10 parts of powdered carboxyl nitrile rubber, 120-140 parts of an inorganic flame retardant, 5-15 parts of a polyphosphazene flame retardant, 3-6 parts of a montmorillonite synergistic flame retardant, 1.5-3 parts of a composite antioxidant, 5-8 parts of a processing aid, and 3-5 parts of an environmentally friendly masterbatch; the polymer matrix comprises 3-5 parts of ethylene-vinyl acetate copolymer grafted with maleic anhydride by radiation and / or 3-5 parts of nylon 12 elastomer grafted with maleic anhydride by radiation, 30-50 parts of ethylene-vinyl acetate copolymer with a low vinyl acetate content, and / or 40-60 parts of ethylene-vinyl acetate copolymer elastomer with a high vinyl acetate content.
2. The wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material according to claim 1, characterized in that: The inorganic flame retardant includes any one or more of silane-treated magnesium hydroxide and silane-treated aluminum hydroxide; the polyphosphazene flame retardant includes hexaphenoxy cyclotriphosphazene and phenoxy polyphosphazene; the composite antioxidant includes a primary antioxidant and an auxiliary antioxidant, wherein the primary antioxidant includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, pentaerythritol tetrakis(3-laurylthiopropionate), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl, N,N'-bis[β-(3 , any one or more of 5-di-tert-butyl-4-hydroxyphenyl)propionyl] hydrazine, the auxiliary antioxidant includes any one or more of the thioester antioxidants thiodipropionate didodecyl ester and thiodipropionate di(octadecyl) ester; the processing aid includes a cross-linking sensitizer and a lubricant, the cross-linking sensitizer includes any one or more of trimethylolpropane trimethacrylate and triallyl isocyanurate, and the lubricant includes any one or more of polyethylene wax, zinc stearate, ethylene bisstearamide and silicone masterbatch.
3. The wear-resistant, halogen-free, low-smoke, flame-retardant polyolefin cable material according to claim 2, characterized in that: The weight ratio of silane-treated magnesium hydroxide to silane-treated aluminum hydroxide in the inorganic flame retardant is 60-80:40-60; the weight ratio of hexaphenoxy cyclotriphosphazene to phenoxy polyphosphazene in the polyphosphazene flame retardant is 5-15:0-4; the weight ratio of the main antioxidant to the auxiliary antioxidant in the composite antioxidant is 1:1-3; the industrial auxiliary agent includes 1-2 parts of a cross-linking sensitizer and 3-5 parts of a lubricant.
4. The wear-resistant, halogen-free, low-smoke, flame-retardant polyolefin cable material according to claim 1, characterized in that: The average particle size of the montmorillonite synergistic flame retardant is 16-22 μm.
5. The method for preparing the wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: putting weighed polymer substrate, powdered carboxyl nitrile rubber, inorganic flame retardant, polyphosphazene flame retardant, montmorillonite synergistic flame retardant, composite antioxidant, processing aid and environmentally friendly masterbatch into an internal mixer for mixing, melting and mixing at a temperature range of 140-160°C, and then transferring to a two-stage twin-screw extruder for air-cooled extrusion granulation at a temperature range of 130-170°C to obtain wear-resistant halogen-free low-smoke flame-retardant polyolefin cable material.
6. The method for preparing the wear-resistant halogen-free, low-smoke, flame-retardant polyolefin cable material according to claim 5, characterized in that: The radiation grafted maleic anhydride ethylene-vinyl acetate copolymer is prepared according to the following steps: 2-5 parts of maleic anhydride are dissolved in acetone, and mixed with 100 parts of ethylene-vinyl acetate copolymer in a high-speed mixer, and after the acetone is completely volatilized, granulation is performed in a twin-screw extruder at 100-130° C. water ring, and then radiation grafting is performed in an electron accelerator at 3-5Mev, and the irradiation dose is 10-25kGy, to obtain 1-3% grafting rate and ≤10% gel content of ethylene-vinyl acetate radiation grafted maleic anhydride ethylene-vinyl acetate copolymer. Ester copolymer; the radiation grafted maleic anhydride nylon 12 elastomer is prepared by the following method: 2-5 parts of maleic anhydride are dissolved in acetone, mixed with 100 parts of nylon 12 elastomer in a high-speed mixer, and after the acetone is completely volatilized, granulated in a twin-screw extruder at 200-230°C water ring, and then radiation grafted in an electron accelerator at 3-5Mev, with an irradiation dose of 10-25kGy, to obtain a radiation grafted maleic anhydride nylon 12 elastomer with a grafting rate of 1-3% and a gel content of ≤10%.
7. Use of the wear-resistant, halogen-free, low-smoke, flame-retardant polyolefin cable material according to any one of claims 1 to 4, characterized in that: The wear-resistant, halogen-free, low-smoke, flame-retardant polyolefin cable material is extruded and coated on the conductor core on a wire and cable extruder production line at a temperature of 120-160°C; then radiation cross-linking is carried out in an electron accelerator with an energy of 1.5-5Mev, an irradiation dose of 100-150kGy, and thermal extension is controlled at 20-40%.