High-strength PEVA netted cloth for trampoline

By using modified bamboo fibers and flame retardants in PEVA mesh cloth, the problems of flammability and insufficient UV resistance are solved, the flame retardant and mechanical properties of the material are improved, and the service life is extended. It also reduces toxicity and meets environmental protection requirements.

CN118931030AInactive Publication Date: 2024-11-12HANGZHOU TRANSASIA SPORTING GOODS MFR CO LTD

Patent Information

Application Number
CN202411190758.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing EVA mesh cloth is flammable and has insufficient UV resistance, which has fire safety hazards and mechanical properties, which is particularly prominent when used outdoors.

Method used

Using high-strength PEVA mesh cloth fabric, the raw materials of LDPE and EVA are modified by mixing matrix resins of LDPE and EVA, modified bamboo fibers, ammonium polyphosphate and expandable graphite flame retardants, alkaline magnesium sulfate whiskers, aluminum borate whiskers and other raw materials. The vibrant bamboo fibers are treated with sodium hydroxide solution and KH550 to enhance the binding of fibers to resin, increase interfacial adhesion, and enhance the flame retardant and mechanical properties of the material through blending and whisker distribution.

Benefits of technology

It improves the material's ultraviolet resistance, flame retardant effect and mechanical properties, extends its service life, and reduces toxicity, meets environmental protection requirements, and reduces potential harm to humans and the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931030A_ABST
    Figure CN118931030A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength PEVA netted sandwich cloth for a trampoline, and relates to the technical field of netted sandwich cloth, the high-strength PEVA netted sandwich cloth comprises the following raw materials by weight: 90-120 parts of matrix resin, 6-10 parts of a flexibilizer, 15-20 parts of a flame retardant, 12-18 parts of mixed whiskers, and 1-2 parts of a pigment. According to the high-strength PEVA netted cloth for the trampoline, part of cellulose, lignin and the like on the surfaces of bamboo fibers are removed through an alkaline solution, hydrogen bonds are formed in molecules, the fiber structure is arranged in order, due to the erosion effect of the alkaline solution, many irregular groove marks and pits are formed in the surfaces of the fibers, gullies on the surfaces of the bamboo fibers are deepened, and the surface roughness of the bamboo fibers is improved. The contact area of the bamboo fibers and the matrix resin is increased, the bamboo fibers are more easily infiltrated by the resin, and the combination of the resin and the matrix resin is facilitated, so that better stress interlocking is formed between the bamboo fibers and the matrix resin, the stress of the composite material can be better transferred to the fibers from the resin, and the mechanical property of the composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mesh cloth, in particular to a high-strength PEVA mesh cloth material for a trampoline. Background Art

[0002] Trampoline mesh cloth is a kind of amusement equipment fabric made of PVC mesh cloth. Trampoline mesh cloth is a professional air-molded cloth with excellent tensile and tear resistance, flame retardant and antioxidant functions. It is widely used not only in children's entertainment trampolines, but also in various inflatable toys and air-molded products.

[0003] PVC needs to be added with specific additives before it is converted into products. These additives play a vital role in the flexibility, stability, color, transparency and electrical properties of PVC products. However, some PVC additives are extremely harmful to human health and the environment, such as cadmium-based and lead-based stabilizers and certain phthalates, which are now restricted by the EU REACH regulations. , There are also potential risks from some PVC additives such as medium-chain chlorinated paraffins and flame retardants 。

[0004] The Chinese patent with publication number CN101225606A discloses an EVA mesh cloth, which is made by heating and compounding high-strength polyester fiber cloth and EVA film; the process is: the two layers of EVA film are preheated and melted by adjusting the temperature of the heating roller, and then pressed with the middle layer of preheated high-strength polyester mesh cloth by rubber rollers and iron rollers, and then cooled and shaped. The EVA mesh cloth of the present invention has simple raw materials, and the manufactured product is non-toxic and environmentally friendly, has high heat resistance, and does not deform when working in a hot environment; it has a long service life and low cost; it can be used in large quantities for handbags, shower curtains, curtains, laundry bags and other household items, and is an excellent material to replace PVC.

[0005] The above-mentioned prior art solutions have the following defects: First, EVA is a non-carbon-forming polymer, which is highly flammable and cannot self-extinguish in an air environment, so there is a fire safety hazard when in use; Second, for a trampoline placed outdoors, it will be exposed to the sun when the outdoor temperature is high, which means that if its ultraviolet resistance is insufficient, long-term exposure will affect its mechanical properties, thereby causing a safety hazard; To this end, the present invention provides a high-strength PEVA mesh cloth for a trampoline to solve the above problems. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a high-strength PEVA mesh cloth for a trampoline, which solves the problems mentioned in the above background technology.

[0007] To achieve the above purpose, the present invention is implemented by the following technical scheme: a high-strength PEVA mesh cloth for a trampoline, comprising the following raw materials in parts by weight: 90 to 120 parts of a base resin, 6 to 10 parts of a toughening agent, 15 to 20 parts of a flame retardant, 12 to 18 parts of a mixed whisker, and 1 to 2 parts of a pigment;

[0008] The matrix resin is a mixture of LDPE and EVA; the toughening agent is a mixture of modified bamboo fiber and maleic anhydride grafted polyethylene; the flame retardant is a mixture of ammonium polyphosphate and expandable graphite; the mixed whiskers include basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers;

[0009] Wherein, the specific modification method of the modified bamboo fiber is:

[0010] S1. After drying the bamboo fiber, place it in a 5% by mass sodium hydroxide solution and soak it for 10 to 12 hours;

[0011] S2, filter again and wash with distilled water until neutral;

[0012] S3, then placed in a drying oven to dry;

[0013] S4, take out and soak in 3% KH550 solution;

[0014] S5. Then pour in the coupling agent and continue soaking at room temperature for 1.5 to 2.5 hours;

[0015] S6. Finally, place the mixture in a drying oven for drying to obtain the modified bamboo fiber.

[0016] Preferably, in S3 and S6, the temperature in the drying box is 75-80° C., and the drying time is 10-12 hours.

[0017] Preferably, the components in the modified bamboo fiber are in the following mass ratios: 2 to 5 parts of bamboo fiber, 40 to 100 parts of sodium hydroxide solution, 40 to 100 parts of KH550 solution, and 40 to 80 parts of coupling agent.

[0018] Preferably, in S5, the coupling agent is prepared by mixing ethanol and water, and then adding a regulator to adjust the pH value to 3.5-4.5.

[0019] Preferably, the mass ratio of the ethanol to water is 1:(0.8-1), and the regulator is glacial acetic acid.

[0020] Preferably, the mass ratio of LDPE to EVA is 1:(3-4).

[0021] Preferably, the mass ratio of the modified bamboo fiber to the maleic anhydride grafted polyethylene is (0.3-0.4):1.

[0022] Preferably, the mass ratio of the ammonium polyphosphate to the expandable graphite is 3:(2-2.4).

[0023] Preferably, the mass ratio of the basic magnesium sulfate whiskers, the aluminum borate whiskers and the calcium sulfate whiskers is 13:(6.5-7):(6.5-7).

[0024] Beneficial Effects

[0025] The present invention provides a high-strength PEVA mesh cloth for a trampoline. Compared with the prior art, it has the following beneficial effects:

[0026] (1) The trampoline uses high-strength PEVA mesh cloth. The cellulose and lignin on the surface of the bamboo fiber are partially removed by an alkaline solution, and hydrogen bonds are formed between the molecules, so that the fiber structure is arranged regularly. Due to the erosion of the alkaline solution, there are more irregular grooves and pits on the fiber surface, which deepens the grooves on the surface of the bamboo fiber and increases the contact area with the matrix resin. The resin is easier to infiltrate the bamboo fiber, which is beneficial to the combination with the matrix resin, so that the bamboo fiber and the matrix resin form a better stress interlocking, and the stress of the composite material can be better transferred from the resin to the fiber, thereby improving the mechanical properties of the composite material. At the same time, since KH550 is a bifunctional compound, it can react with the bamboo fiber and the matrix resin to form a "bridge" between the two, promote the adhesion of the fiber to the matrix resin, enhance the interfacial adhesion between the fiber and the resin, and improve the interfacial compatibility of the composite material.

[0027] (2) The trampoline uses high-strength PEVA mesh fabric, which is blended with EVA and PE. Since EVA contains polar groups, it has good compatibility with other additives and can effectively improve the uniformity of the dispersion of the corresponding additives in PE, thereby improving the elasticity of the fabric, improving the fabric's resistance to stress fracture and flex cracking, improving its resistance to ultraviolet rays, and extending the service life of the fabric.

[0028] (3) The trampoline uses high-strength PEVA mesh cloth. By adding mixed whiskers, the whiskers are staggered and densely bonded to the matrix interface. At the same time, since the pyrolysis products of the whiskers are in a network-like skeleton, they have a reinforcing effect on the carbon layer. Therefore, while improving the flame retardant effect of the material, its mechanical properties can also be improved.

[0029] (4) The trampoline is made of high-strength PEVA mesh fabric, which is low-toxic and biodegradable, and complies with EU PVC Environmental protection requirements for restricted use of materials minimize exposure of humans and the environment to these persistent, potentially bioaccumulative and toxic substances. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The microstructure SEM images of bamboo fiber before and after modification provided for a high-strength PEVA mesh cloth material for a trampoline of the present invention;

[0031] Figure 2 This is a comparison chart of ultraviolet aging tests of Example 1 and Comparative Example 1 provided for a high-strength PEVA mesh cloth for a trampoline of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In the technical solution, the coupling agent is prepared by mixing ethanol and water in a mass ratio of 1:0.8, then adding glacial acetic acid and adjusting the pH value to 4.

[0034] Example 1

[0035] A high-strength PEVA mesh cloth for a trampoline, the process is:

[0036] Step 1, weighing the raw materials: 90g of a mixture of LDPE and EVA, 10g of a mixture of modified bamboo fiber and maleic anhydride grafted polyethylene, 20g of a mixture of ammonium polyphosphate and expandable graphite, 18g of basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers, and 2g of pigment, wherein the mass ratio of LDPE to EVA is 1:3, the mass ratio of modified bamboo fiber to maleic anhydride grafted polyethylene is 0.3:1, and the mass ratio of basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers is 13:6.5:6.5;

[0037] The specific modification method of the modified bamboo fiber is as follows: 2 parts of bamboo fiber are dried and placed in 100 parts of a sodium hydroxide solution with a mass fraction of 5% for immersion for 10 hours; then filtered and washed with distilled water until neutral; then placed in a drying oven at 75°C for 10 hours; taken out and immersed in 100 parts of a KH550 solution with a mass fraction of 3%; then poured in 80 parts of a coupling agent and continued to be immersed at room temperature for 2 hours; finally placed in a drying oven at 80°C for 10 hours to obtain the modified bamboo fiber;

[0038] Step 2: Pour all raw materials into the mixer and run it at a low speed, raise the temperature to 120°C, discharge the mixed materials into the cold mixing pot, and start the cold mixing process;

[0039] Step 3: Set the temperature of the first twin-screw extruder to 140° C. and keep the constant temperature for 2 hours, then add the mixed material into the first twin-screw extruder, and obtain the plasticized material after shearing by the first twin-screw extruder combination;

[0040] Step 4: Set the temperature of the first single-screw extruder to 140° C. and keep the constant temperature for 2 hours, then pour the plasticized material into the first single-screw extruder;

[0041] Step 5: After extrusion, the pellets are transported to a pelletizer and cut into pellets with a particle size of 8 mm. After impurities are removed, the pellets are transported to a vibrating screen to separate and obtain film blowing pellets.

[0042] Step six, set the temperature of the second twin-screw extruder to 140°C, and the temperature of the second single-screw extruder to 160°C, and keep the constant temperature for 5 hours respectively, add the blown film pellets into the second twin-screw extruder, after molding and plasticizing by the second twin-screw extruder, send them to the second single-screw extruder, and blow mold at the die head of the second single-screw extruder to obtain high-strength PEVA mesh cloth.

[0043] Example 2

[0044] A high-strength PEVA mesh cloth for a trampoline, the process is:

[0045] Step 1, weighing the raw materials: 100g of a mixture of LDPE and EVA, 8g of a mixture of modified bamboo fiber and maleic anhydride grafted polyethylene, 18g of a mixture of ammonium polyphosphate and expandable graphite, 15g of basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers, and 1.5g of pigment, wherein the mass ratio of LDPE to EVA is 1:3.5, the mass ratio of modified bamboo fiber to maleic anhydride grafted polyethylene is 0.4:1, and the mass ratio of basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers is 13:6.5:7;

[0046] The specific modification method of the modified bamboo fiber is as follows: 3 parts of bamboo fiber are dried and placed in 70 parts of sodium hydroxide solution with a mass fraction of 5% for immersion for 11 hours; then filtered and washed with distilled water until neutral; then placed in a drying oven at 80°C for 11 hours; taken out and immersed in 70 parts of KH550 solution with a mass fraction of 3%; then poured in 60 parts of coupling agent and continued to be immersed at room temperature for 2 hours; finally placed in a drying oven at 80°C for 10 hours to obtain the modified bamboo fiber;

[0047] Step 2: Pour all raw materials into the mixer and run it at a low speed, raise the temperature to 120°C, discharge the mixed materials into the cold mixing pot, and start the cold mixing process;

[0048] Step 3: Set the temperature of the first twin-screw extruder to 140° C. and keep the constant temperature for 2 hours, then add the mixed material into the first twin-screw extruder, and obtain the plasticized material after shearing by the first twin-screw extruder combination;

[0049] Step 4: Set the temperature of the first single-screw extruder to 140° C. and keep the constant temperature for 2 hours, then pour the plasticized material into the first single-screw extruder;

[0050] Step 5: After extrusion, the pellets are transported to a pelletizer and cut into pellets with a particle size of 8 mm. After impurities are removed, the pellets are transported to a vibrating screen to separate and obtain film blowing pellets.

[0051] Step six, set the temperature of the second twin-screw extruder to 140°C, and the temperature of the second single-screw extruder to 160°C, and keep the constant temperature for 5 hours respectively, add the blown film pellets into the second twin-screw extruder, after molding and plasticizing by the second twin-screw extruder, send them to the second single-screw extruder, and blow mold at the die head of the second single-screw extruder to obtain high-strength PEVA mesh cloth.

[0052] Example 3

[0053] A high-strength PEVA mesh cloth for a trampoline, the process is:

[0054] Step 1, weighing the raw materials: 120g of a mixture of LDPE and EVA, 6g of a mixture of modified bamboo fiber and maleic anhydride grafted polyethylene, 15g of a mixture of ammonium polyphosphate and expandable graphite, 12g of basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers, and 1g of pigment, wherein the mass ratio of LDPE to EVA is 1:4, the mass ratio of modified bamboo fiber to maleic anhydride grafted polyethylene is 0.4:1, and the mass ratio of basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers is 13:7:6.5;

[0055] The specific modification method of the modified bamboo fiber is as follows: 5 parts of bamboo fiber are dried and placed in 40 parts of sodium hydroxide solution with a mass fraction of 5%, and soaked for 12 hours; then filtered and washed with distilled water until neutral; then placed in a drying oven at 80°C for 12 hours; taken out and soaked in 40 parts of KH550 solution with a mass fraction of 3%; then poured in 40 parts of coupling agent and continued to soak at room temperature for 2 hours; finally placed in a drying oven at 80°C for 10 hours to obtain the modified bamboo fiber;

[0056] Step 2: Pour all raw materials into the mixer and run it at a low speed, raise the temperature to 120°C, discharge the mixed materials into the cold mixing pot, and start the cold mixing process;

[0057] Step 3: Set the temperature of the first twin-screw extruder to 140° C. and keep the constant temperature for 2 hours, then add the mixed material into the first twin-screw extruder, and obtain the plasticized material after shearing by the first twin-screw extruder combination;

[0058] Step 4: Set the temperature of the first single-screw extruder to 140° C. and keep the constant temperature for 2 hours, then pour the plasticized material into the first single-screw extruder;

[0059] Step 5: After extrusion, the pellets are transported to a pelletizer and cut into pellets with a particle size of 8 mm. After impurities are removed, the pellets are transported to a vibrating screen to separate and obtain film blowing pellets.

[0060] Step six, set the temperature of the second twin-screw extruder to 140°C, and the temperature of the second single-screw extruder to 160°C, and keep the constant temperature for 5 hours respectively, add the blown film pellets into the second twin-screw extruder, after molding and plasticizing by the second twin-screw extruder, send them to the second single-screw extruder, and blow mold at the die head of the second single-screw extruder to obtain high-strength PEVA mesh cloth.

[0061] Comparative Example 1

[0062] The high-strength PEVA mesh cloth for a trampoline provided in this comparative example is substantially the same as that in Example 1, the main difference is that in this comparative example 1, the modified bamboo fiber in Example 1 is replaced with unmodified bamboo fiber.

[0063] Comparative Example 2

[0064] The high-strength PEVA mesh cloth for a trampoline provided in this comparative example is substantially the same as that in Example 1, the main difference is that in this comparative example 1, the ammonium polyphosphate and expandable graphite in Example 1 are replaced with ammonium polyphosphate.

[0065] Comparative Example 3

[0066] The high-strength PEVA mesh cloth for a trampoline provided in this comparative example is substantially the same as that in Example 1, the main difference is that in this comparative example 1, the basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers in Example 1 are replaced with basic magnesium sulfate whiskers.

[0067] UV aging test: Place the sample in a UV aging box for testing. Test conditions: temperature 60°C, cumulative radiation dose UV30kwh / m 2 、UV60kwh / m 2 , of which UVA is 93% and UVB is 7%.

[0068] like Figure 2 As shown, cracks appear on the surface of the sample of Comparative Example 1, while the surface of the sample of Example 1 is intact and still maintains good mechanical properties, indicating that the sample of Example 1 has better anti-ultraviolet aging performance.

[0069] like Figure 1 As shown in the figure, the surface of the unmodified bamboo fiber is rough and has a lot of colloid attached to it. After modification, an obvious deposition layer is formed on the surface of the bamboo fiber, which has a good coating effect and promotes interface fusion. The gaps between single fibers are enlarged, looser, and the grooves are deepened, which is convenient for the matrix resin to infiltrate the fibers, greatly reducing the polarity of the bamboo fiber surface and improving the compatibility of the two-phase interface of the composite material.

[0070] Vertical combustion test: According to GB / T8332-2008, the evaluation standard of the test results is U-94 standard, and the vertical combustion test is carried out using CZF-3 horizontal / vertical combustion tester; according to the test standard of the vertical combustion test, the flame retardant grade is divided into three grades: V-0, V-1, and V-2; the results are shown in Table 1.

[0071] Limiting oxygen index test: According to GB / T2406-2008, the JF-3 limiting oxygen index tester produced by Nanjing Jiangning District Analytical Instrument Factory was used; the results are shown in Table 1.

[0072] Tensile strength test: According to GB / T 1446-2005, the sample was placed on a standard tool and punched into a dumb-shaped shape, and then measured on a WD-10E electronic universal testing machine at a temperature of 23°C and a tensile speed of 2 mm / min. The results are shown in Table 1.

[0073] Tear strength test: According to GB / T 3917.2, the sample was placed on a universal testing machine for testing; the results are shown in Table 1.

[0074] Table 1

[0075]

[0076] In the present technical solution, expandable graphite expands rapidly after being heated, and its volume can reach ten or even a hundred times of its original size, and the expanded layer formed has good thermal stability, thereby inhibiting the combustion process of the material. However, it will produce a "wick effect" during the flame retardant process, that is, it will form a "worm"-like layer, causing the fire source to drip like a candle when burning, transferring heat and causing other parts of the material to burn, affecting its flame retardant effect. Therefore, ammonium polyphosphate and expandable graphite are compounded. Under their synergistic effect, the "wick effect" can be avoided, and they can also work together physically. When added in small amounts, they have a good flame retardant effect.

[0077] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0078] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-strength PEVA mesh cloth for a trampoline, characterized in that: The invention comprises the following raw materials in parts by weight: 90 to 120 parts of base resin, 6 to 10 parts of toughening agent, 15 to 20 parts of flame retardant, 12 to 18 parts of mixed whiskers, and 1 to 2 parts of pigment; The matrix resin is a mixture of LDPE and EVA; the toughening agent is a mixture of modified bamboo fiber and maleic anhydride grafted polyethylene; the flame retardant is a mixture of ammonium polyphosphate and expandable graphite; the mixed whiskers include basic magnesium sulfate whiskers, aluminum borate whiskers and calcium sulfate whiskers; Wherein, the specific modification method of the modified bamboo fiber is: S1. After drying the bamboo fiber, place it in a 5% by mass sodium hydroxide solution and soak it for 10 to 12 hours; S2, filter again and wash with distilled water until neutral; S3, then placed in a drying oven to dry; S4, take out and soak in 3% KH550 solution; S5. Then pour in the coupling agent and continue soaking at room temperature for 1.5 to 2.5 hours; S6. Finally, place the mixture in a drying oven for drying to obtain the modified bamboo fiber.

2. The high-strength PEVA mesh cloth for a trampoline according to claim 1, characterized in that: In S3 and S6, the temperature in the drying box is 75-80° C., and the drying time is 10-12 hours.

3. The high-strength PEVA mesh cloth for a trampoline according to claim 1, characterized in that: The components in the modified bamboo fiber are in the following weight ratios: 2 to 5 parts of bamboo fiber, 40 to 100 parts of sodium hydroxide solution, 40 to 100 parts of KH550 solution, and 40 to 80 parts of coupling agent.

4. The high-strength PEVA mesh cloth for a trampoline according to claim 1, characterized in that: In S5, the coupling agent is prepared by mixing ethanol and water, and then adding a regulator to adjust the pH value to 3.5-4.

5.

5. The high-strength PEVA mesh cloth for a trampoline according to claim 4, characterized in that: The mass ratio of the ethanol to water is 1:(0.8-1), and the regulator is glacial acetic acid.

6. The high-strength PEVA mesh cloth for a trampoline according to claim 1, characterized in that: The mass ratio of LDPE to EVA is 1:(3-4).

7. The high-strength PEVA mesh cloth for a trampoline according to claim 1, characterized in that: The mass ratio of the modified bamboo fiber to the maleic anhydride grafted polyethylene is (0.3-0.4):

1.

8. The high-strength PEVA mesh cloth for a trampoline according to claim 1, characterized in that: The mass ratio of the ammonium polyphosphate to the expandable graphite is 3:(2-2.4).

9. The high-strength PEVA mesh cloth for a trampoline according to claim 1, characterized in that: The mass ratio of the basic magnesium sulfate whisker, the aluminum borate whisker and the calcium sulfate whisker is 13:(6.5-7):(6.5-7).

Citation Information

Patent Citations

  • EVA composite material, as well as EVA composite clip net cloth and preparation method thereof

    CN104558801A