Organic modified expanded graphite composite polymer wave-absorbing material and preparation method thereof

By adhering the synergistic effect of modified expanded graphite and internal flame retardant on the surface of conductive polymer foam particles, the problem of insufficient mechanical properties and flame retardant properties of wave absorbing materials is solved, and high mechanical strength and high power tolerance are achieved.

CN118931033APending Publication Date: 2024-11-12WUXI FREGEP ABSORBING MATERIAL TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410981853.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing wave absorbing materials have shortcomings in high mechanical properties and flame retardant properties, especially in military vehicles and aircraft camouflage applications, which have fragile mechanical properties, poor flame retardant properties, and are prone to deformation or fire in high-power radiation environments.

Method used

Using organic modified expanded graphite composite polymer absorbing material, the mechanical strength and continuous wave resistance power performance of the material are improved by adhering to the surface of conductive polymer foam particles and combining the synergistic effect of internal flame retardants. .

Benefits of technology

The mechanical strength and flame retardant properties of the wave absorbing material are significantly improved, and the resistance power is maintained at a high power environment to be increased to more than 2500W, and the electromagnetic parameter performance is optimized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931033A_ABST
    Figure CN118931033A_ABST
Patent Text Reader

Abstract

The invention provides an organic modified expanded graphite composite polymer wave-absorbing material and a preparation method thereof, and belongs to the technical field of wave-absorbing materials, the wave-absorbing material comprises conductive polymer foam particles and modified expanded graphite attached to the surfaces of the conductive polymer foam particles, 0.5-20kg of modified expanded graphite is attached to the surface of each cubic meter of conductive polymer foam particles. According to the absorption principle of the organic modified expanded graphite composite polymer wave-absorbing material, electromagnetic waves are converted into heat to be dissipated, when the conductive polymer foam particles are of an annular structure, due to the fact that the surface area of the particles is large, more organic modified expanded graphite can be adhered under the condition that compression molding of the particles is not affected, and the wave-absorbing effect is good. The oxygen index is greatly improved, the tolerance power of the annular polymer wave-absorbing material can be improved to be larger than 2500W by the annular structure in a high-power test, and the heat dissipation effect of the annular polymer wave-absorbing material is superior to that of a wave-absorbing material formed by pressing solid foam particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wave absorbing materials, and in particular to an organic modified expanded graphite composite polymer wave absorbing material and a preparation method thereof. Background Art

[0002] In the application fields of microwave darkrooms, military vehicles, and aircraft camouflage, the microwave darkroom absorbing materials have very high requirements for flame retardancy and withstand power, while the absorbing materials used for military vehicles and aircraft camouflage have high requirements for flame retardancy and even higher requirements for the mechanical properties of the absorbing materials. At present, the absorbing materials used for military vehicles and aircraft camouflage are mainly made of thermosetting polyurethane, thermosetting adhesives, composite wood-cut glass fiber pressed plates, but due to their brittle mechanical properties, the vibrations during high-speed flight of aircraft, vehicle driving, and door opening and closing often cause the absorbing materials to break and fall off.

[0003] When high-power testing is required in a microwave darkroom, the continuous wave power radiation density that ordinary sponge absorbing materials can withstand is about 1200W. Due to the high water absorption rate of sponges, when the water content in the air is high on rainy days, the electromagnetic parameters of the sponge change greatly, which has a great impact on the performance of the darkroom.

[0004] The continuous wave power radiation density of traditional polystyrene foam absorbing materials is about 800W. Since polystyrene foam has good adhesive adhesion, thermoplastic adhesives are usually used to mix absorbents and flame retardants to coat the surface of foam particles and then press them into absorbing materials. However, polystyrene foam itself has poor mechanical strength and poor temperature resistance. When the temperature exceeds 80°C, the material will deform and shrink.

[0005] Conventional flame-retardant polypropylene or polyethylene foam absorbing materials can withstand a power radiation density of about 1200W in continuous waves. When the power radiation density exceeds the tolerable power radiation density, the absorbing materials with insufficient mechanical strength will deform and fall off, and will catch fire when the flame retardancy is poor. In order to improve the flame retardancy, if a thermoplastic adhesive is used to mix an absorbent and a flame retardant to coat the surface of polypropylene and polyethylene foam particles, and then pressed into an absorbing material, the adhesive has poor adhesion to the surface of polypropylene or polyethylene foam, and there is a layer of adhesive between the foam balls, which will cause the mechanical strength of the absorbing material to be seriously reduced. The fracture surface of the broken material is observed, and the fracture is torn between the foam balls. Generally, the temperature resistance of thermoplastic adhesives is lower than that of polypropylene and polyethylene foams themselves. Therefore, if the absorbing material is bonded by thermoplastic adhesives, its continuous wave withstand power radiation density is less than 1200W.

[0006] The currently manufactured polypropylene or polyethylene absorbing materials have different oil absorption values, iodine absorption values ​​and specific surface areas of carbon black, graphite and conductive agents of different specifications. Even if the same type of conductive agent powder is added in the same proportion, different extrusion processes can lead to different dispersion effects, resulting in large differences in resistance. The electromagnetic parameter performance of the final absorbing material will also be quite different. Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an organic modified expanded graphite composite polymer absorbing material and a preparation method thereof. Due to the unique and reliable flame retardant mechanism of expanded graphite, a low softening point organic material is used to coat the surface of expanded graphite, and a certain proportion of modified expanded graphite is adhered to the surface of conductive polymer foam particles by a hot melt method. While ensuring the flame retardant performance of the absorbing material, no matter how much the density of the polymer foam particles is, 0.5-20 kg / m3 of conductive polymer foam particles are adhered to the surface of each cubic meter of conductive polymer foam particles. 3 Expanded graphite, the flame retardant inside the conductive polymer foam particles and the modified expanded graphite on the surface work synergistically, which can not only solve the high oxygen index problem of the conductive polymer foam absorbing material, but also greatly improve the mechanical strength and continuous wave withstand power performance of the polymer foam absorbing material.

[0008] The technical solution adopted by the present invention is as follows:

[0009] An organic modified expanded graphite composite polymer absorbing material comprises conductive polymer foam particles and modified expanded graphite attached to the surface of the conductive polymer foam particles, wherein 0.5-20 kg of modified expanded graphite is attached to the surface of each cubic meter of conductive polymer foam particles.

[0010] Preferably, the organic modified expanded graphite composite polymer absorbing material comprises, by weight, 60-93 parts of expanded graphite, 2-40 parts of low softening point organic material, 0.1-20 parts of plasticizer, 0.1-25 parts of conductive agent and 0.1-5 parts of coupling agent.

[0011] Preferably, the organic modified expanded graphite composite polymer absorbing material, wherein: the low softening point organic material is selected from one or more of polyvinyl butyral, polyvinyl acetate, acrylic resin, modified acrylic resin, maleic anhydride grafted ethylene acrylic acid copolymer, ethylene acrylic acid copolymer, phenolic resin, aromatic modified terpene resin, dammar resin, aldehyde ketone resin, chlorinated polypropylene, chloroacetic acid resin, and soluble polyurethane.

[0012] Preferably, the organically modified expanded graphite composite polymer absorbing material, wherein: the conductive polymer foam particles are selected from one of conductive polypropylene foam particles and conductive polyethylene foam particles, the shape of the conductive polymer foam particles is selected from one of columnar, annular and spherical, the resistance of the conductive polymer foam particles is 300 ohms-200M ohms, and the particle size is 1-6mm, the particle size includes diameter and length, and the diameter and length of the conductive polymer foam particles are both within the range of 1-6mm.

[0013] Preferably, the organically modified expanded graphite composite polymer absorbing material, wherein: by weight, the conductive polymer foam particles include 5-70 parts of polypropylene or polyethylene resin with a melting point greater than 120°C, 30-90 parts of conductive masterbatch, 2-30 parts of flame retardant masterbatch, 0.1-2 parts of nucleating agent masterbatch, and 0.3-1 parts of antioxidant masterbatch.

[0014] Preferably, in the organically modified expanded graphite composite polymer absorbing material, the resistance of the conductive masterbatch is 10 ohms to 200K ohms.

[0015] Preferably, the organically modified expanded graphite composite polymer absorbing material, wherein: the flame retardant masterbatch comprises 40-60% of polypropylene or polyethylene resin and 40-60% of flame retardant, by mass percentage, and the flame retardant is selected from one or more of aluminum phosphate, zinc phosphate, aluminum tripolyphosphate, hydroxyethylidene diphosphonic acid, aluminum dihydrogen phosphate, ammonium polyphosphate, pentaerythritol aluminum phosphate, coated red phosphorus, decabromodiphenylethane, and brominated polystyrene.

[0016] The present invention also provides a method for preparing an organic modified expanded graphite composite polymer absorbing material, which comprises the following steps:

[0017] Step S1. By weight, 60-93 parts of expanded graphite are added to a mixer, the temperature of the mixer is controlled to be 80-100°C, then 0.1-5 parts of a coupling agent are diluted with a solvent and sprayed onto the surface of the expanded graphite and dried, then 2-40 parts of a low softening point organic material are dissolved with a solvent, and 0.1-20 parts of a plasticizer and 0.1-25 parts of a conductive agent are added to obtain a mixed solution, and finally the mixed solution is sprayed onto the surface of the stirred expanded graphite with a timed automatic sprayer, and dried to obtain modified expanded graphite;

[0018] Step S2. 5-70 parts of polypropylene or polyethylene resin, 30-90 parts of conductive masterbatch, 2-30 parts of flame retardant masterbatch, 0.1-2 parts of nucleating agent masterbatch, and 0.3-1 parts of antioxidant masterbatch are mixed and extruded through a twin-screw extruder to obtain polymer microparticles;

[0019] Step S3. Put the polymer microparticles prepared in step S2 into a reactor, add water and a dispersant, then heat and introduce carbon dioxide until the target temperature and pressure are reached for foaming, then release the material and wash it, and finally dry it to obtain conductive polymer foam particles;

[0020] Step S4. Add the conductive polymer foam particles obtained in step S3 into a mixer, control the temperature of the mixer to 100-120° C., then add modified expanded graphite and stir, and then cool to obtain a composite material;

[0021] Step S5. The composite material obtained in step S4 is molded by a foam molding machine to obtain an absorbing material.

[0022] Preferably, in the method for preparing the organically modified expanded graphite composite polymer absorbing material, the solvent in step S1 is one or more of water, ethanol, n-butanol, ethyl acetate, acetone, toluene, xylene, butyl acetate, cyclohexanone, isopentyl acetate, ethylene glycol ethyl ether acetate, and ammonia water.

[0023] Preferably, the method for preparing the organically modified expanded graphite composite polymer absorbing material, wherein: in step S2, the polymer microparticles are one of columnar microparticles, annular microparticles, and spherical microparticles. When the polymer microparticles are columnar microparticles, the resistance of the polymer microparticles is 50 ohms-200K ohms, the particle length is 0.5-5mm, and the diameter is 0.5-2mm; when the polymer microparticles are annular microparticles, the resistance of the polymer microparticles is 50 ohms-200K ohms, the inner diameter is 0.1-0.5mm, the outer diameter is 0.6-2mm, and the length is 1-5mm; when the polymer microparticles are spherical microparticles, the resistance of the polymer microparticles is 50 ohms-200K ohms, and the diameter is 0.5-1.8mm.

[0024] The advantages of the present invention are:

[0025] (1) In the organic modified expanded graphite composite polymer absorbing material and the preparation method thereof described in the present invention, the flame retardant masterbatch inside the conductive polymer foam particles and the modified expanded graphite on the surface not only solve the high oxygen index problem of the conductive polymer foam particles in the molded manufacturing of absorbing materials through synergistic effect, but also because the modified expanded graphite is evenly and discontinuously distributed on the surface of the foam particles, there is no organic adhesive that completely covers the surface of the foam particles. When the foam particles are steam-heated and extruded inside the mold of the foam molding machine, the fusion property and conductive continuity of the foam particles are not affected. At the same time, the organic material on the surface of the organic modified expanded graphite is also melted with the surface of the foam particles, which greatly improves the mechanical strength and power tolerance performance of the composite material molded manufacturing absorbing material.

[0026] (2) The absorption principle of the absorbing material is to convert electromagnetic waves into heat and dissipate it. In the organic modified expanded graphite composite polymer absorbing material and the preparation method thereof described in the present invention, when the conductive polymer foam particles are annular in structure, the surface area of ​​the particles is large. Without affecting the particle compression molding, more modified expanded graphite can be adhered, which can not only greatly improve the oxygen index, but also the heat dissipation effect of the annular particle absorbing material is much better than that of the absorbing material pressed by solid foam particles. In the high-power test, the annular structure can increase the tolerable power of the annular polymer absorbing material to more than 2500W. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the SEM image of the composite material prepared in Example 1.

[0028] Figure 2 This is the SEM image of the composite material prepared in Example 2.

[0029] Figure 3 This is a SEM image of the composite material prepared in Example 2 after being cut open.

[0030] Figure 4 This is a schematic diagram of a flat-plate absorbing material with grooves on the surface prepared in Example 1-2.

[0031] Figure 5 for Figure 4 A partial enlarged view of the part indicated by circle A. DETAILED DESCRIPTION

[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and examples. Unless otherwise specified, the terms used herein should be understood according to the conventional usage of ordinary technicians in the field.

[0033] As used herein, the low softening point organic material is an organic material having a glass transition temperature below 100°C. The low softening point organic material has good flexibility. When hot-melt attached to polymer foam particles, the foam particles will not melt and have good adhesion. The preferred low softening point organic material in this application is one or more of polyvinyl butyral, polyvinyl acetate, acrylic resin, modified acrylic resin, maleic anhydride grafted ethylene acrylic acid copolymer, ethylene acrylic acid copolymer, phenolic resin, aromatic modified terpene resin, dammar resin, aldehyde ketone resin, chlorinated polypropylene, chloroacetic acid resin, and soluble polyurethane.

[0034] Preferably, the low softening point organic material of the polymer microparticles described in the present invention is one or more of acrylic resin, modified acrylic resin, maleic anhydride grafted ethylene acrylic acid copolymer, aromatic modified terpene resin, ethylene acrylic acid copolymer, and chlorinated polypropylene.

[0035] As used in this article, the continuous wave power resistance performance refers to a microwave signal with a continuous waveform, and its frequency is usually between 1GHz and 100GHz. When electromagnetic waves are continuously emitted, high requirements are placed on the temperature resistance and flame retardancy of the material. When electromagnetic waves are continuously emitted, the material will continue to heat up and generate heat without a cooling process. The absorbing material can convert most of the incident electromagnetic waves into heat energy and dissipate it, and a small part will be transmitted. The continuous heat accumulation can melt or burn the absorbing material.

[0036] As used herein, the polymer microparticles are microparticles obtained by mixing polypropylene or polyethylene resin with a melting point greater than 120°C, conductive masterbatch, flame retardant masterbatch, nucleating agent masterbatch, and antioxidant masterbatch and extruding through a twin-screw extruder. The melting point is the critical temperature when a solid substance is converted into a liquid, and is the specific temperature at which a crystalline substance is converted from a solid state to a liquid state; the polymer microparticles are one of columnar microparticles, annular microparticles, and spherical microparticles. When the polymer microparticles are columnar microparticles, their resistance is 50 ohms-200K ohms, the particle length is 0.5-5mm, and the diameter is 0.5-2mm; when the polymer microparticles are annular microparticles, their resistance is 50 ohms-200K ohms, the inner diameter is 0.1-0.5mm, the outer diameter is 0.6-2mm, and the length is 1-5mm; when the polymer microparticles are spherical microparticles, their resistance is 50 ohms-200K ohms, and the diameter is 0.5-1.8mm. By extruding the polymer microparticles into an annular structure, the power tolerance performance of the absorbing material can be improved.

[0037] Preferably, when the polymer microparticles described in the present invention are columnar microparticles, the particle length is 1-4 mm and the diameter is 0.8-1 mm; when the polymer microparticles are annular microparticles, the inner diameter is 0.2-0.4 mm, the outer diameter is 0.8-1.5 mm, and the length is 2-4 mm; when the polymer microparticles are spherical microparticles, the diameter is 0.8-1 mm.

[0038] Preferably, the conductive polymer foam particles of the present invention have a resistance of 300 ohms to 200 M ohms and a particle size of 1-6 mm. The particle size includes diameter and length, and the diameter and length of the conductive polymer foam particles are both within the range of 1-6 mm, preferably with a diameter of 1.5-2 mm and a length of 2-3 mm. A smaller particle size can increase the total particle number and total surface area of ​​the foam particles per cubic meter, and the more foam particles there are, the larger the total surface area is, the more dispersed the fixed mass of organically modified expanded graphite attached to the surface of the foam particles is, and the more dispersed the organically modified expanded graphite is, the less influence it has on foam molding.

[0039] The modified expanded graphite of the present invention comprises 60-93 parts of expanded graphite, 2-40 parts of low softening point organic material, 0.1-20 parts of plasticizer, 0.1-25 parts of conductive agent and 0.1-5 parts of coupling agent. Wherein, if the expanded graphite is not modified, it cannot adhere to the surface of polypropylene and polyethylene resin foam particles, so it is necessary to modify the expanded graphite first, so that a layer of organic material with good adhesion to polypropylene and polyethylene foam is attached to the surface of the expanded graphite, so that the expanded graphite can adhere to the surface of polypropylene and polyethylene foam particles. The preferred low softening point organic material of the present invention is selected from one or more of polyvinyl butyral, polyvinyl acetate, acrylic resin, modified acrylic resin, maleic anhydride grafted ethylene acrylic acid copolymer, ethylene acrylic acid copolymer, phenolic resin, aromatic modified terpene resin, dammar resin, aldehyde ketone resin, chlorinated polypropylene, chloroacetic acid resin and soluble polyurethane.

[0040] The modified expanded graphite of the present invention is adhered to the surface of the conductive polymer foam particles and cooled to obtain a composite material. The composite material can be cut open and then subjected to SEM testing to observe the surface morphology of the composite material and detect the quality of the obtained composite material.

[0041] Example 1

[0042] A method for preparing an organic modified expanded graphite composite polymer absorbing material comprises the following steps:

[0043] Step S1. 85 kg of expanded graphite is added to a ribbon mixer, the temperature of the mixer is controlled to be 100 ° C, 5 kg of KH-550 coupling agent is subsequently diluted with 5 kg of ethanol, and then the dilution is sprayed on the surface of the expanded graphite and dried, 20 kg of acrylic resin is dissolved with 200 kg of ammonia water, 5 kg of diethyl phthalate, 2 kg of carbon black, and 0.2 kg of Dow Corning defoamer AFE3168 are added, and a mixed solution is obtained, the pH value of the ammonia water is greater than 12, and the mixed solution is slowly sprayed on the surface of the stirred expanded graphite with a timed automatic sprayer, and dried to obtain modified expanded graphite;

[0044] Step S2. 8 kg of polypropylene resin with a melting point greater than 130°C, 85 kg of polypropylene conductive masterbatch with a resistance of 80 ohms, 15 kg of polypropylene flame retardant masterbatch, 1 kg of zinc borate nucleating agent masterbatch, and 1 kg of aromatic amine antioxidant masterbatch are mixed and extruded through a twin-screw extruder to obtain polymer microparticles with a resistance of 160 ohms, a particle length of 3 mm, and a diameter of 1 mm;

[0045] In terms of mass percentage, the polypropylene conductive masterbatch comprises 60% polypropylene, 32% conductive carbon black and 8% PE wax; the polypropylene flame retardant masterbatch comprises 60% polypropylene and 40% coated red phosphorus; the zinc borate nucleating agent masterbatch comprises 85% polypropylene, 10% zinc borate and 5% PE wax; the aromatic amine antioxidant masterbatch comprises 10% 1010 antioxidant, 85% polypropylene and 5% PE wax;

[0046] Step S3. Put the polymer microparticles into a reactor, add 70% of the total volume of the reactor with water and 3% of the total mass of the polymer microparticles with sodium dodecylbenzene sulfonate, then heat to the melting point of the polymer, and slowly introduce carbon dioxide several times until the pressure reaches 4Mpa for foaming, then release the material and wash it, and dry it to obtain a material with a resistance of 1800 ohms, a diameter of 2.5mm, a length of 4mm, and a density of 45kg / m 3 Conductive polymer foam particles;

[0047] Step S4. 45 kg of conductive polymer foam particles are added to the mixer, and the temperature of the mixer is controlled to be 120 ° C. When the material temperature reaches 120 ° C, 10 kg of modified expanded graphite is added and continued to stir at a stirring speed of 35 r / min for 5 min. The modified expanded graphite adheres to the surface of the conductive polymer foam particles and is cooled to obtain a composite material.

[0048] Step S5. The composite material is molded by a foam molding machine to obtain a flat-plate absorbing material with a thickness of 25 mm and grooves on the surface.

[0049] Example 2

[0050] A method for preparing an organic modified expanded graphite composite polymer absorbing material comprises the following steps:

[0051] Step S1. 85 kg of expanded graphite is added to a ribbon mixer, the temperature of the mixer is controlled to be 100 ° C, 5 kg of KH-550 coupling agent is diluted with 5 kg of ethanol and sprayed on the surface of the expanded graphite and dried, 20 kg of acrylic resin is dissolved with 200 kg of ammonia water, 5 kg of diethyl phthalate, 2 kg of carbon black, and 0.2 kg of Dow Corning defoamer AFE3168 are added, and a mixed solution is obtained, the pH value of the ammonia water is greater than 12, and the mixed solution is slowly sprayed on the surface of the stirred expanded graphite with a timed automatic sprayer, and dried to obtain modified expanded graphite;

[0052] Step S2. 8 kg of polypropylene resin with a melting point greater than 130° C., 85 kg of polypropylene conductive masterbatch with a resistance of 80 ohms, 15 kg of polypropylene flame retardant masterbatch, 1 kg of zinc borate nucleating agent masterbatch, and 1 kg of aromatic amine antioxidant masterbatch are mixed and extruded through a twin-screw extruder to obtain polymer microparticles with a resistance of 160 ohms, a particle length of 3 mm, an inner diameter of 0.3 mm, and an outer diameter of 1 mm. The polymer microparticles are in the shape of ring-shaped microparticles;

[0053] In terms of mass percentage, the polypropylene conductive masterbatch comprises 60% polypropylene, 32% conductive carbon black and 8% PE wax; the polypropylene flame retardant masterbatch comprises 60% polypropylene and 40% coated red phosphorus; the zinc borate nucleating agent masterbatch comprises 85% polypropylene, 10% zinc borate and 5% PE wax; the aromatic amine antioxidant masterbatch comprises 10% 1010 antioxidant, 85% polypropylene and 5% PE wax;

[0054] Step S3. Put the polymer microparticles into a reactor, add 70% of the total volume of the reactor with water and 3% of the total mass of the polymer microparticles with sodium dodecylbenzene sulfonate, then heat to the melting point of the polymer, and introduce carbon dioxide to a pressure of 4 MPa for foaming, then release the material and wash it, and dry it to obtain a material with a resistance of 1800 ohms, an outer diameter of 3.5 mm, an inner diameter of 1.6 mm, a length of 4 mm, and a density of 35 kg / m 3 Ring-shaped conductive polypropylene foam particles;

[0055] Step S4. 35 kg of conductive polymer foam particles were added to the mixer, the temperature of the mixer was controlled to be 120 ° C, and then 10 kg of modified expanded graphite was added and continued to stir at a stirring speed of 35 r / min for 5 min. The modified expanded graphite adhered to the surface of the conductive polymer foam particles and cooled to obtain a composite material;

[0056] Step S5. The composite material is molded by a foam molding machine to obtain a flat-plate absorbing material with a thickness of 25 mm and grooves on the surface.

[0057] Comparative Example 1

[0058] A method for preparing an organic modified expanded graphite composite polymer absorbing material comprises the following steps:

[0059] Step S1. 8 kg of polypropylene resin with a melting point greater than 130°C, 85 kg of polypropylene conductive masterbatch with a resistance of 80 ohms, 15 kg of polypropylene flame retardant masterbatch, 1 kg of zinc borate nucleating agent masterbatch, and 1 kg of aromatic amine antioxidant masterbatch are mixed and extruded through a twin-screw extruder to obtain polymer microparticles with a resistance of 160 ohms, a particle length of 3 mm, and a diameter of 1 mm;

[0060] In terms of mass percentage, the polypropylene conductive masterbatch comprises 60% polypropylene, 32% conductive carbon black and 8% PE wax; the polypropylene flame retardant masterbatch comprises 60% polypropylene and 40% coated red phosphorus; the zinc borate nucleating agent masterbatch comprises 85% polypropylene, 10% zinc borate and 5% PE wax; the aromatic amine antioxidant masterbatch comprises 10% 1010 antioxidant, 85% polypropylene and 5% PE wax;

[0061] Step S2. Put the polymer microparticles into a reactor, add 70% of the total volume of the reactor with water and 3% of the total mass of the polymer microparticles with sodium dodecylbenzene sulfonate, then heat to the melting point of the polymer, introduce carbon dioxide to a pressure of 4 MPa, release the material, wash it, and dry it to obtain a material with a resistance of 1800 ohms, a diameter of about 2.5 mm, a length of about 4 mm, and a density of 45 kg / m 3 Conductive polymer foam particles;

[0062] Step S3. The conductive polymer foam particles are molded by a foam molding machine to obtain a flat-plate absorbing material with a thickness of 25 mm and grooves on the surface.

[0063] Comparative Example 2

[0064] A method for preparing an organic modified expanded graphite composite polymer absorbing material comprises the following steps:

[0065] Step S1. 85 kg of expanded graphite is added to a ribbon mixer, the temperature of the mixer is controlled to be 100 ° C, 5 kg of KH-550 coupling agent is subsequently diluted with 5 kg of ethanol, and then the dilution is sprayed onto the surface of the expanded graphite and dried, 20 kg of acrylic resin is dissolved with 200 kg of ammonia water, 5 kg of diethyl phthalate, 2 kg of carbon black, and 0.2 kg of Dow Corning defoamer AFE3168 are added, and a mixed solution is obtained, wherein the pH value of the ammonia water is greater than 12, and the mixed solution is slowly sprayed onto the surface of the stirred expanded graphite with a timed automatic sprayer, and dried to obtain modified expanded graphite;

[0066] Step S2. 8 kg of polypropylene resin with a melting point greater than 130°C, 85 kg of polypropylene conductive masterbatch with a resistance of 80 ohms, 15 kg of polypropylene flame retardant masterbatch, 1 kg of zinc borate nucleating agent masterbatch, and 1 kg of aromatic amine antioxidant masterbatch are mixed and extruded through a twin-screw extruder to obtain polymer microparticles with a resistance of 160 ohms, a particle length of 3 mm, and a diameter of 1 mm;

[0067] In terms of mass percentage, the polypropylene conductive masterbatch comprises 60% polypropylene, 32% conductive carbon black and 8% PE wax; the polypropylene flame retardant masterbatch comprises 60% polypropylene and 40% coated red phosphorus; the zinc borate nucleating agent masterbatch comprises 85% polypropylene, 10% zinc borate and 5% PE wax; the aromatic amine antioxidant masterbatch comprises 10% 1010 antioxidant, 85% polypropylene and 5% PE wax;

[0068] Step S3. Put the polymer microparticles into a reactor, add 70% of the total volume of the reactor with water and 3% of the total mass of the polymer microparticles with sodium dodecylbenzene sulfonate, then heat to the melting point of the polymer, and slowly introduce carbon dioxide several times until the pressure is 4 MPa, release the material and wash it, and dry it to obtain a material with a resistance of 1800 ohms, a diameter of about 2.5 mm, a length of about 4 mm, and a density of 45 kg / m 3 Conductive polymer foam particles;

[0069] Step S4. 45 kg of conductive polymer foam particles were added to the mixer, the temperature of the mixer was controlled to be 120 ° C, and then 25 kg of modified expanded graphite was added and continued to stir at a stirring speed of 35 r / min for 5 min. The modified expanded graphite adhered to the surface of the conductive polymer foam particles and cooled to obtain a composite material;

[0070] Step S5. The composite material is molded by a foam molding machine to obtain a flat-plate absorbing material with a thickness of 25 mm and grooves on the surface.

[0071] The absorbing materials of Examples 1 and 2 and Comparative Examples 1 and 2 were tested, and the test results are shown in Table 1 below.

[0072] Table 1

[0073]

[0074]

[0075] It can be seen from Table 1 above that in Example 1, modified expanded graphite is added according to the method of the present invention, and the mechanical properties do not change, but the flame retardant properties are greatly improved.

[0076] Comparative Example 1 is a fire hazard due to its poor flame retardant performance.

[0077] In Comparative Example 2, since the surface of the foam particles is coated with more expanded graphite, too much modified expanded graphite exists on the surface of the foam particles, causing the modified expanded graphite to fall off more seriously. The foam particles cannot be welded together by their own materials, but are welded together by the low softening point organic material on the surface. Therefore, during the high power test, when the temperature reaches the glass transition temperature of the low softening point organic material, the foam begins to deform and collapse.

[0078] Example 2 is an absorbing material made of annular polymer foam particles, in which organic modified expanded graphite is added and prepared according to the method described in the present invention, without affecting the welding performance of the material itself. Due to the 2.5 cm thick plate and the annular foam particle structure, the overall air permeability and heat dissipation performance of the foam is good, so the withstand power can be increased to more than 2500W.

[0079] Further, according to Figure 1 It can be seen from the SEM image of the composite material prepared in Example 1 that the modified expanded graphite adheres to the surface of the solid conductive polymer foam particles, and there is no low softening point organic material attached to the place where the modified expanded graphite is not adhered, which does not affect the steam molding of the foam particles. The particle surface has a certain roughness, which can improve the adhesion of the modified expanded graphite to the surface of the conductive polymer foam particles.

[0080] Further, according to Figure 2 The SEM image of the composite material prepared in Example 2 is shown as well as Figure 3 From the SEM image of the composite material prepared in Example 2 after being cut, it can be seen that modified expanded graphite is attached to the inside and surface of the annular conductive polymer foam particles, and no low-softening-point organic material is attached to the places where the modified expanded graphite is not attached, which does not affect the steam molding of the conductive polymer foam particles; after the annular foam particles are cut, the bubbles are evenly distributed along the arc, the annular structure has a good heat dissipation effect, and the organic modified expanded graphite is attached to the surface of the annular particles, and synergistically acts with the internal added flame retardant, thereby greatly improving the flame retardancy and power tolerance performance of the absorbing material.

[0081] Figure 4 and Figure 5 This is a schematic diagram of a flat-plate absorbing material with grooves on the surface prepared in Example 1-2, which illustrates that the surface of the absorbing material is designed with a frequency selective surface structure. The surface is designed with regular grooved grids, so that the flat-plate absorbing material has a good absorption rate in a wide frequency band.

[0082] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, ordinary technicians in the field should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. An organic modified expanded graphite composite polymer absorbing material, characterized in that: The invention comprises conductive polymer foam particles and modified expanded graphite attached to the surface of the conductive polymer foam particles, wherein 0.5-20 kg of modified expanded graphite is attached to the surface of each cubic meter of conductive polymer foam particles.

2. The organic modified expanded graphite composite polymer absorbing material according to claim 1, characterized in that: In parts by weight, the modified expanded graphite includes 60-93 parts of expanded graphite, 2-40 parts of low softening point organic material, 0.1-20 parts of plasticizer, 0.1-25 parts of conductive agent and 0.1-5 parts of coupling agent.

3. The organic modified expanded graphite composite polymer absorbing material according to claim 2, characterized in that: The low softening point organic material is selected from one or more of polyvinyl butyral, polyvinyl acetate, acrylic resin, modified acrylic resin, maleic anhydride grafted ethylene acrylic acid copolymer, ethylene acrylic acid copolymer, phenolic resin, aromatic modified terpene resin, dammar resin, aldehyde ketone resin, chlorinated polypropylene, chloroacetic acid resin, and soluble polyurethane.

4. The organic modified expanded graphite composite polymer absorbing material according to claim 1, characterized in that: The conductive polymer foam particles are selected from conductive polypropylene foam particles and conductive polyethylene foam particles. The shape of the conductive polymer foam particles is selected from columnar, annular and spherical. The conductive polymer foam particles have a resistance of 300 ohms to 200 M ohms and a particle size of 1-6 mm.

5. The organic modified expanded graphite composite polymer absorbing material according to claim 4, characterized in that: By weight, the conductive polymer foam particles include 5-70 parts of polypropylene or polyethylene resin with a melting point greater than 120° C., 30-90 parts of conductive masterbatch, 2-30 parts of flame retardant masterbatch, 0.1-2 parts of nucleating agent masterbatch, and 0.3-1 parts of antioxidant masterbatch.

6. The organic modified expanded graphite composite polymer absorbing material according to claim 5, characterized in that: The electrical resistance of the conductive masterbatch is 10 ohms to 200K ohms.

7. The organic modified expanded graphite composite polymer absorbing material according to claim 5, characterized in that: In terms of mass percentage, the flame retardant masterbatch comprises 40-60% of polypropylene or polyethylene resin and 40-60% of flame retardant, wherein the flame retardant is selected from one or more of aluminum phosphate, zinc phosphate, aluminum tripolyphosphate, hydroxyethylidene diphosphonic acid, aluminum dihydrogen phosphate, ammonium polyphosphate, pentaerythritol aluminum phosphate, coated red phosphorus, decabromodiphenylethane, and brominated polystyrene.

8. The method for preparing the organic modified expanded graphite composite polymer absorbing material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step S1. By weight, 60-93 parts of expanded graphite are added to a mixer, the temperature of the mixer is controlled to be 80-100° C., then 0.1-5 parts of a coupling agent are diluted with a solvent and sprayed onto the surface of the expanded graphite and dried, then 2-40 parts of a low softening point organic material are dissolved with a solvent, and 0.1-20 parts of a plasticizer and 0.1-25 parts of a conductive agent are added to obtain a mixed solution, and finally the mixed solution is sprayed onto the surface of the stirred expanded graphite with an automatic sprayer, and dried to obtain modified expanded graphite; Step S2. 5-70 parts of polypropylene or polyethylene resin, 30-90 parts of conductive masterbatch, 2-30 parts of flame retardant masterbatch, 0.1-2 parts of nucleating agent masterbatch, and 0.3-1 parts of antioxidant masterbatch are mixed and extruded through a twin-screw extruder to obtain polymer microparticles; Step S3. Put the polymer microparticles prepared in step S2 into a reactor, add water and a dispersant, then heat and introduce carbon dioxide until the target temperature and pressure are reached for foaming, then release the material and wash it, and finally dry it to obtain conductive polymer foam particles; Step S4. Add the conductive polymer foam particles obtained in step S3 into a mixer, control the temperature of the mixer to 100-120° C., then add modified expanded graphite and stir, and then cool to obtain a composite material; Step S5. The composite material obtained in step S4 is molded by a foam molding machine to obtain an absorbing material.

9. The method for preparing the organic modified expanded graphite composite polymer absorbing material according to claim 8, characterized in that: In step S1, the solvent is one or more of water, ethanol, n-butanol, ethyl acetate, acetone, toluene, xylene, butyl acetate, cyclohexanone, isopentyl acetate, ethylene glycol ethyl ether acetate, and aqueous ammonia.

10. The method for preparing the organic modified expanded graphite composite polymer absorbing material according to claim 8, characterized in that: The polymer microparticles prepared in step S2 are one of columnar microparticles, annular microparticles, and spherical microparticles. When the polymer microparticles are columnar microparticles, the resistance of the polymer microparticles is 50 ohms-200K ohms, the particle length is 0.5-5mm, and the diameter is 0.5-2mm; when the polymer microparticles are annular microparticles, the resistance of the polymer microparticles is 50 ohms-200K ohms, the inner diameter is 0.1-0.5mm, the outer diameter is 0.6-2mm, and the length is 1-5mm; when the polymer microparticles are spherical microparticles, the resistance of the polymer microparticles is 50 ohms-200K ohms, and the diameter is 0.5-1.8mm.

Citation Information

Patent Citations

  • Wave absorbing material and preparation method thereof

    CN106519471A

  • Polystyrene foam wave-absorbing sphere with core-shell structure and preparation method thereof

    CN113444283A

  • Foaming wave-absorbing material combining polypropylene and metal micro-nano particles and preparation method of foaming wave-absorbing material

    CN115873347A

  • Surface-polarized modified polystyrene foam wave-absorbing material and preparation method thereof

    CN117164933A

  • Preparation method of wave-absorbing flame-retardant brown PMI (polymethacrylimide) composite foam