Wear-resistant, corrosion-resistant and high-temperature-resistant rubber sealing material for oil field and preparation method thereof

By introducing the blending of vinyl functionalized POSS and EPDM into the oil field sealing materials, a stable cross-linking network is formed, which solves the problems of oxidative degradation and thermal aging of ethylene propylene rubber at high temperatures, and significantly improves the wear resistance of the material and high temperature resistance, extend service life and enhance chemical corrosion resistance.

CN118931052AInactive Publication Date: 2024-11-12JIANGSU GREENSTAR ECO RUBBER TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411216860.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing oilfield sealing materials show problems such as degradation of mechanical properties, insufficient wear resistance and shortened service life in high temperature, high pressure and strong corrosion environments. Especially ethylene propylene rubber oxidation degradation and thermal aging at high temperatures, resulting in its Seal performance deteriorates in complex chemical environments.

Method used

Use vinyl functionalized POSS as a modified component to blend it with EPDM substrate to form a composite rubber sealing material. The double bond cross-linking of vinyl functionalized POSS and EPDM is formed to form a stable three-dimensional cross-linking network to improve cross-link density and molecules Chain strength and enhance the wear resistance and high temperature resistance of the material by introducing fluorine, epoxy and silane groups.

Benefits of technology

It significantly improves the material's wear resistance, high temperature resistance and chemical corrosion resistance, extends its service life, and maintains good mechanical properties and sealing properties in high-temperature and high-pressure environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005021770250000021
    Figure BDA0005021770250000021
  • Figure BDA0005021770250000141
    Figure BDA0005021770250000141
  • Figure BDA0005021770250000151
    Figure BDA0005021770250000151
Patent Text Reader

Abstract

The invention relates to the technical field of sealing materials, and particularly provides a wear-resistant, corrosion-resistant and high-temperature-resistant rubber sealing material for an oil field and a preparation method of the rubber sealing material. The sealing material comprises the following raw materials: EPDM, vinyl functionalized POSS, a vulcanizing agent, a filler, a plasticizer, an accelerant and an antioxidant, octavinyl POSS is subjected to graft modification by adopting trifluoropropyl trichlorosilane so as to obtain vinyl functionalized POSS, and the nano functional material is adopted to enhance the performance of an EPDM rubber composite material, so that the sealing material has good sealing performance. The wear resistance, the corrosion resistance and the high-temperature resistance can be remarkably improved, so that the high-temperature-resistant wear-resistant steel has a good application prospect in oil field equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing materials, and in particular to a wear-resistant, corrosion-resistant and high-temperature-resistant rubber sealing material for oil fields and a preparation method thereof. Background Art

[0002] In the process of oil field development, sealing materials need to work in high temperature, high pressure, strong corrosion and high wear environment. Although the existing sealing materials are excellent in some aspects, they are still insufficient in comprehensive performance. For example, fluororubber (FKM) is expensive, hydrogenated nitrile rubber (HNBR) is expensive and has limited high temperature resistance, and polytetrafluoroethylene (PTFE) is not as good as elastomeric materials in mechanical properties and wear resistance.

[0003] The chemical structure of EPDM contains a saturated main chain structure, which gives it excellent resistance to oxidation, ozone and corrosion. Among all rubbers, EPDM has the lowest specific gravity. It can absorb a large amount of fillers and oils without much effect on its properties. It can be made into low-cost rubber compounds and is widely used in the fields of automobiles, construction and electricity. However, the structure of its side chains is prone to oxidative degradation and thermal aging at high temperatures, resulting in a decrease in the mechanical properties of the material and a shortened service life. In addition, the wear resistance of EPDM is also affected by its molecular structure and cross-linking density. Although EPDM has good elasticity, the strength and cross-linking density of its molecular chain are lower than those of other high-performance rubbers such as HNBR. Therefore, in a high-wear environment, the surface of EPDM is easily worn, resulting in rapid wear and aging of the material. The ethylene and propylene monomers contained in the chemical structure of EPDM have good tolerance to polar chemicals such as acids and alkalis, but poor tolerance to non-polar chemicals and organic solvents. In a complex chemical environment, EPDM is prone to swelling and degradation, resulting in a decrease in the mechanical properties and sealing performance of the material. In addition, high temperature and high pressure environment will intensify the erosion of EPDM by chemical media, further reducing its chemical corrosion resistance.

[0004] In view of its low cost and good weather resistance, there are endless modifications for EPDM, but there are relatively few reports on the introduction of modified POSS into EPDM through blending. Octavinyl POSS is an organic-inorganic hybrid structural material, and the rigid Si-O-Si structure provides unique heat resistance and excellent mechanical properties. On the other hand, the organic groups connected to the Si vertex group can improve the compatibility and vulcanization time of POSS with the EPDM matrix, significantly increase its crosslinking density, significantly increase its glass transition temperature, and reduce its thermal expansion coefficient, which significantly improves the thermal stability and mechanical properties of EPDM products. Summary of the invention

[0005] In view of this, the present invention aims to solve the above technical problems and provide a wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields and a preparation method thereof.

[0006] The technical solution of the present invention is achieved as follows: The present invention provides a wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields, which adopts EPDM as a substrate and vinyl functionalized POSS as a key modified component to prepare a composite rubber sealing material in order to obtain good wear resistance, corrosion resistance and high-temperature resistance. The raw materials of the rubber sealing material are calculated by weight and include:

[0007]

[0008] In some embodiments, the preparation method of vinyl-functionalized POSS includes: dissolving octavinyl POSS in dichloromethane, adding chloroplatinic acid, stirring and mixing evenly, slowly dropping trifluoropropyltrichlorosilane under a nitrogen atmosphere, and after the dropwise addition, stirring and reacting at 30-40°C for 4-6h, filtering and drying to obtain vinyl-functionalized POSS, wherein the molar ratio of vinyl POSS to trifluoropropyltrichlorosilane is 1:(2-3).

[0009] In some embodiments, in the preparation method of vinyl functionalized POSS, while slowly dropping trifluoropropyltrichlorosilane, it also includes slowly dropping glycidyltrimethoxysilane, and the molar ratio of vinyl POSS to glycidyltrimethoxysilane is 1:(2-3).

[0010] In some embodiments, in the preparation method of vinyl functionalized POSS, while slowly dropping trifluoropropyltrichlorosilane, it also includes slowly dropping trimethoxysilane, and the molar ratio of vinyl POSS to trimethoxysilane is 1:(2-3).

[0011] In some embodiments, the vulcanizing agent is sulfur.

[0012] In some embodiments, the filler is carbon black.

[0013] In some embodiments, the plasticizer is paraffin oil.

[0014] In some embodiments, the feed agent is CBS or TTBS.

[0015] In some embodiments, the antioxidant is a RD antioxidant.

[0016] In addition, the present invention also provides a method for preparing the above-mentioned wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields, which specifically comprises the following steps:

[0017] Step 1, premixing and dispersing EPDM with vinyl functionalized POSS, filler, plasticizer and antioxidant;

[0018] Step 2: The premixed and dispersed materials in step 1 are subjected to shear mixing treatment for 5-10 minutes by a twin-screw extruder at 100-120° C. and 200-300 rpm;

[0019] Step 3: Mix the sheared mixed material obtained in step 2 with the vulcanizer and the accelerator, add them into an open mill and continue to mix them evenly, then put them into a mold, and perform molding treatment at 150-180°C for 10-30min to obtain a sealing material; the roll temperature of the open mill is 60-80°C, the roll distance is 1.5-2mm, the roll speed is 20-30rpm, and the mixing time is 3-5min.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention adopts EPDM as a substrate and adopts polysilsesquioxane, an organic-inorganic hybrid material with a cage structure, as a modified material, thereby significantly improving the comprehensive performance of EPDM. Specifically, vinyl-functionalized POSS is adopted as a functional modified material, which has a plurality of reactive vinyl groups and can be cross-linked with double bonds of EPDM to form a stable three-dimensional cross-linked network. The introduction of POSS increases the cross-linking density and molecular chain strength of EPDM, thereby significantly improving the wear resistance of the material. The inorganic silicon-oxygen structure of POSS has good thermal stability, thereby improving the high temperature resistance of EPDM and reducing the oxidative degradation and thermal aging of the material at high temperatures. Furthermore, the fluorine group introduced into the functionalized POSS has extremely low surface energy and high chemical inertness, thereby significantly improving the tolerance of the material to non-polar chemicals and organic solvents. Furthermore, by introducing an epoxy group, the cross-linking density and mechanical strength can be increased, and the wear resistance can be improved. The introduction of a silane group enhances the high temperature resistance of the material and the binding property with the matrix. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.

[0024] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.

[0025] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0026] The molecular chain strength and cross-linking density of EPDM are lower than those of other high-performance rubbers (such as HNBR). In a high-wear environment, the surface is easily worn, resulting in rapid wear and aging of the material. The unsaturated double bonds on the side chains of EPDM make it prone to oxidative degradation and thermal aging at high temperatures, resulting in a decrease in the mechanical properties of the material and a shortened service life. High temperatures will accelerate the cross-linking of the material and the breakage of the molecular chain, thereby affecting its high-temperature resistance. In addition, EPDM has poor tolerance to non-polar chemicals and organic solvents. In a complex chemical environment, EPDM is more likely to swell and degrade, resulting in a decrease in the mechanical properties and sealing performance of the material. High temperature and high pressure environments will intensify the erosion of EPDM by chemical media, further reducing its chemical corrosion resistance.

[0027] The present application adopts vinyl-functionalized POSS, which can significantly improve the wear resistance, high temperature resistance and chemical corrosion resistance of EPDM. Since POSS has a cage-like structure with high rigidity and stability, after the introduction of POSS, nano-scale hard particles are formed in the rubber matrix, and these hard particles are distributed in the flexible EPDM group to form a high-resolution composite structure of rigid and flexible materials, thereby improving the wear resistance of the material. Among them, the vinyl-functionalized POSS forms cross-linking points by copolymerizing with the double bonds of EPDM, which significantly increases the cross-linking density of the rubber. The high cross-linking density improves the mechanical strength and wear resistance of the material and reduces the wear of the material in a friction environment.

[0028] At the same time, the silicon oxygen cage structure of POSS has excellent thermal stability and can withstand high temperatures without degradation. This thermal stability can improve the high temperature resistance of the overall material by dispersing it in the EPDM matrix.

[0029] Fluorine groups have extremely low surface energy and high chemical inertness, which can significantly improve the material's tolerance to non-polar chemicals and organic solvents. They are introduced into POSS molecules through hydrogen silanization reaction, giving them extremely low surface energy and high chemical inertness. By introducing this fluorine-based POSS into the EPDM matrix, the swelling and degradation of EPDM in non-polar chemicals can be reduced, significantly improving the material's resistance to chemical corrosion.

[0030] Epoxy groups are introduced into POSS molecules through cycloaddition reactions, making them highly reactive. Epoxy groups can react with active groups in EPDM to form cross-linked bonds, thereby increasing the cross-linking density of the material. The increase in cross-linking density significantly enhances the mechanical strength and rigidity of the material, reduces wear on the material surface during friction, and improves wear resistance.

[0031] Silane is introduced into the POSS molecule through hydrolysis and condensation reaction, making it better bonded with the matrix material.

[0032] The silane group undergoes a condensation reaction with the hydroxyl or amine group in EPDM to form a Si-O-Si bond, which has extremely high thermal stability and can remain stable at high temperatures, reducing thermal degradation of the material.

[0033] The technical solution of the present application is described in detail below through specific embodiments.

[0034] Example 1

[0035] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0036] Preparation of fluorinated vinyl functionalized POSS:

[0037] Dissolve 50g of octavinyl POSS (0.0789mol) in 1L of dichloromethane, add 50mg of chloroplatinic acid, stir at 30°C, keep the reaction system under nitrogen atmosphere, slowly add 36.2g of trifluoropropyltrichlorosilane (0.1578mol), maintain 30°C after the addition, stir and react for 6h, filter and dry under reduced pressure to obtain fluorine-containing vinyl functionalized POSS.

[0038] Preparation of sealant materials:

[0039] 100g EPDM, 5g fluorine-containing vinyl functionalized POSS, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0040] Example 2

[0041] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0042] Preparation of Vinyl-functionalized POSS Containing Fluorine and Epoxy Groups:

[0043] Dissolve 50g of octavinyl POSS (0.0789mol) in 1L of dichloromethane, add 50mg of chloroplatinic acid, stir at 30°C, keep the reaction system under nitrogen atmosphere, slowly add 36.2g of trifluoropropyltrichlorosilane (0.1578mol) and 39.7g of epoxypropyltrimethoxysilane (0.1578mol), maintain 30°C after the addition, stir and react for 6h, filter and dry under reduced pressure to obtain fluorine-containing vinyl functionalized POSS.

[0044] Preparation of sealant materials:

[0045] 100g EPDM, 5g fluorine- and epoxy-containing vinyl functionalized POSS, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0046] Example 3

[0047] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0048] Preparation of Vinyl-functionalized POSS Containing Fluorine and Silane Groups:

[0049] Dissolve 50g of octavinyl POSS (0.0789mol) in 1L of dichloromethane, add 50mg of chloroplatinic acid, stir at 30°C, keep the reaction system under nitrogen atmosphere, slowly add 36.2g of trifluoropropyltrichlorosilane (0.1578mol) and 16.45g of trimethoxysilane (0.1578mol), maintain 30°C after the addition, stir and react for 6h, filter and dry under reduced pressure to obtain fluorine-containing vinyl functionalized POSS.

[0050] Preparation of sealant materials:

[0051] 100g EPDM, 5g vinyl functionalized POSS containing fluorine and silane groups, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0052] Example 4

[0053] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0054] Preparation of Vinyl-functionalized POSS Containing Fluorine, Epoxy and Silane Groups:

[0055] Dissolve 50g of octavinyl POSS (0.0789mol) in 1L of dichloromethane, add 50mg of chloroplatinic acid, stir at 30°C, keep the reaction system under nitrogen atmosphere, slowly add 36.2g of trifluoropropyltrichlorosilane (0.1578mol), 39.7g of epoxypropyltrimethoxysilane (0.1578mol) and 16.45g of trimethoxysilane (0.1578mol), after the addition is completed, maintain 30°C, stir the reaction for 6h, filter and dry under reduced pressure to obtain fluorine-containing vinyl functionalized POSS.

[0056] Preparation of sealant materials:

[0057] 100g EPDM, 5g vinyl functionalized POSS containing fluorine and silane groups, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0058] Example 5

[0059] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0060] Preparation of fluorinated vinyl functionalized POSS:

[0061] Dissolve 50g of octavinyl POSS (0.0789mol) in 1L of dichloromethane, add 50mg of chloroplatinic acid, stir at 40°C, keep the reaction system under nitrogen atmosphere, slowly add 54.3g of trifluoropropyltrichlorosilane (0.2367mol), maintain 40°C after the addition, stir and react for 4h, filter and dry under reduced pressure to obtain fluorine-containing vinyl functionalized POSS.

[0062] Preparation of sealant materials:

[0063] 100g EPDM, 5g fluorine-containing vinyl functionalized POSS, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0064] Example 6

[0065] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0066] Preparation of fluorinated vinyl functionalized POSS:

[0067] Dissolve 50g of octavinyl POSS (0.0789mol) in 1L of dichloromethane, add 50mg of chloroplatinic acid, stir at 30°C, keep the reaction system under nitrogen atmosphere, slowly add 36.2g of trifluoropropyltrichlorosilane (0.1578mol), maintain 30°C after the addition, stir and react for 6h, filter and dry under reduced pressure to obtain fluorine-containing vinyl functionalized POSS.

[0068] Preparation of sealant materials:

[0069] 100g EPDM, 10g fluorine-containing vinyl functionalized POSS, 70g carbon black N330, 20g paraffin oil and 2g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 200rpm for 10min at 120°C. Then, the treated mixture was mixed with 3g sulfur and 2g accelerator TTBS and added to an open mill for mixing. The roll temperature of the open mill was 80°C, the roll distance was 2mm, and the roll speed was 30rpm. After the open mill treatment for 5min, the mixture was placed in a mold and molded at 150°C for 30min to obtain a sealing material.

[0070] Example 7

[0071] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0072] Preparation of fluorinated vinyl functionalized POSS:

[0073] Dissolve 50g of octavinyl POSS (0.0789mol) in 1L of dichloromethane, add 50mg of chloroplatinic acid, stir at 30°C, keep the reaction system under nitrogen atmosphere, slowly add 36.2g of trifluoropropyltrichlorosilane (0.1578mol), maintain 30°C after the addition, stir and react for 6h, filter and dry under reduced pressure to obtain fluorine-containing vinyl functionalized POSS.

[0074] Preparation of sealant materials:

[0075] 100g EPDM, 8g fluorine-containing vinyl functionalized POSS, 60g carbon black N330, 15g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 2g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 60°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 5min, the mixture was placed in a mold and molded at 180°C for 20min to obtain a sealing material.

[0076] Comparative Example 1

[0077] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0078] Preparation of sealant materials:

[0079] 100g EPDM, 5g octavinyl POSS, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0080] Comparative Example 2

[0081] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0082] Preparation of sealant materials:

[0083] 100g EPDM, 55g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100℃. Then the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70℃, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170℃ for 20min to obtain a sealing material.

[0084] Comparative Example 3

[0085] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0086] Preparation of sealant materials:

[0087] 100g EPDM, 3g octavinyl POSS, 2g trifluoropropyl trichlorosilane, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0088] Comparative Example 4

[0089] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0090] Preparation of sealant materials:

[0091] 100g EPDM, 2g octavinyl POSS, 1.5g trifluoropropyl trichlorosilane, 1.5g epoxypropyl trimethoxysilane, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0092] Comparative Example 5

[0093] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0094] Preparation of sealant materials:

[0095] 100g EPDM, 2.5g octavinyl POSS, 1.7g trifluoropropyl trichlorosilane, 0.8g trimethoxysilane, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0096] Comparative Example 6

[0097] This embodiment provides an EPDM-based sealant material, and the preparation method thereof is as follows:

[0098] Preparation of sealant materials:

[0099] 100g EPDM, 1.7g octavinyl POSS, 1.2g trifluoropropyl trichlorosilane, 1.4g epoxypropyl trimethoxysilane, 0.7g trimethoxysilane, 50g carbon black N330, 10g paraffin oil and 1g RD antioxidant were weighed respectively, mixed and stirred for pre-dispersion, and then added to a twin-screw extruder, and shear mixing was carried out at 250rpm for 5min at 100°C. Then, the treated mixture was mixed with 2g sulfur and 1g accelerator CBS and added to an open mill for mixing. The roll temperature of the open mill was 70°C, the roll distance was 1.5mm, and the roll speed was 20rpm. After the open mill treatment for 3min, the mixture was placed in a mold and molded at 170°C for 20min to obtain a sealing material.

[0100] The sealing materials obtained in the above embodiments and comparative examples were respectively subjected to wear resistance test, high temperature resistance test and chemical corrosion resistance test, wherein:

[0101] The wear resistance test is carried out according to ASTM D5963 standard: the specimen is mounted on an abrasion tester and the abrasion test is carried out under the same load and speed. The wear volume (mm) is calculated based on the weight difference before and after abrasion. 3 );

[0102] The high temperature resistance test is carried out according to ASTM D573 standard: in a standard heat aging test chamber at 200℃, the aging treatment is carried out for 72 hours, and then the mechanical properties of the specimens, such as tensile strength, are tested, and the retention rate of mechanical properties before and after heat aging is calculated;

[0103] The chemical corrosion resistance test was carried out according to ASTM D471 standard: the sample was immersed in strong acid (30% sulfuric acid), strong base (10% sodium hydroxide solution), and organic solvent (toluene) for 24 hours, and the weight change of the test material was measured.

[0104] The results of the above tests are shown in the following table:

[0105]

[0106]

[0107] The above-described embodiment data can be seen that the EPDM that the present invention adopts vinyl functionalized POSS to modify has significantly improved in comprehensive performance compared to the EPDM of conventional unmodified vinyl POSS, and after fluorine-based modification, epoxy-modified and silyl-based modification are simultaneously adopted in the best embodiment 4, wear resistance, high temperature resistance and chemical corrosion resistance are compared with only fluorine-based modification of embodiment 1 and the dual modification of embodiment 2 and embodiment 3, all have significantly improved. Simultaneously, by the contrast with comparative example 3-comparative example 6, it can be seen that, when adopting the same raw material, but when not adopting pre-modified vinyl POSS, although various aspects of performance are compared with the EPDM that does not adopt vinyl POSS to have certain improvement, the performance improvement is obviously not as good as the scheme of adopting functionalized vinyl POSS. It can be seen that, by carrying out functionalized modification treatment to vinyl POSS, the performance improvement of EPDM has been played an unexpected technical effect.

[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields, characterized in that: The raw materials of the rubber sealing material are calculated by weight and include:

2. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields according to claim 1, characterized in that: The preparation method of the vinyl functionalized POSS comprises: dissolving octavinyl POSS in dichloromethane, adding chloroplatinic acid, stirring and mixing evenly, slowly dropping trifluoropropyltrichlorosilane under a nitrogen atmosphere, stirring and reacting at 30-40° C. for 4-6 hours after the dropping is completed, filtering and drying to obtain the vinyl functionalized POSS, wherein the molar ratio of the vinyl POSS to the trifluoropropyltrichlorosilane is 1:(2-3).

3. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields as claimed in claim 2, characterized in that: In the preparation method of vinyl functionalized POSS, while slowly dropping trifluoropropyltrichlorosilane, it also includes slowly dropping glycidyltrimethoxysilane, and the molar ratio of vinyl POSS to glycidyltrimethoxysilane is 1:(2-3).

4. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields as claimed in claim 2, characterized in that: In the preparation method of vinyl functionalized POSS, while slowly dropping trifluoropropyltrichlorosilane, trimethoxysilane is also slowly dropped, and the molar ratio of vinyl POSS to trimethoxysilane is 1:(2-3).

5. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields according to claim 1, characterized in that: The vulcanizing agent is sulfur.

6. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields according to claim 1, characterized in that: The filler is carbon black.

7. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields according to claim 1, characterized in that: The plasticizer is paraffin oil.

8. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields according to claim 1, characterized in that: The accelerator is CBS or TTBS.

9. The wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields according to claim 1, characterized in that: The antioxidant is RD antioxidant.

10. The method for preparing the wear-resistant, corrosion-resistant and high-temperature resistant rubber sealing material for oil fields according to any one of claims 1 to 9, characterized in that: The steps include: Step 1, premixing and dispersing EPDM with vinyl functionalized POSS, filler, plasticizer and antioxidant; Step 2: The premixed and dispersed materials in step 1 are subjected to shear mixing treatment for 5-10 minutes by a twin-screw extruder at 100-120° C. and 200-300 rpm; Step 3: Mix the sheared mixed material obtained in step 2 with the vulcanizer and the accelerator, add them into an open mill and continue to mix them evenly, then put them into a mold, and perform molding treatment at 150-180°C for 10-30min to obtain a sealing material; the roll temperature of the open mill is 60-80°C, the roll distance is 1.5-2mm, the roll speed is 20-30rpm, and the mixing time is 3-5min.

Citation Information

Patent Citations

  • Modified fluorine-containing silicone oil and preparation method thereof

    CN104610549A

  • Addition type liquid fluorinated silicone rubber composition and preparation method thereof

    CN111440450A

  • Addition type liquid silicone rubber modified by liquid vinyl polyhedral oligomeric silsesquioxane and preparation method of addition type liquid silicone rubber

    CN115960464A

  • Cage-type polysilsesquioxane simultaneously containing ethyoxyl and fluoro group and preparation method and application of cage-type polysilsesquioxane simultaneously containing ethyoxyl and fluoro group

    CN117417531A

  • Process for continuous production of olefin polyhedral oligomeric silsesquioxane cages

    US20060263318A1