Antibacterial PVC material and preparation method thereof

By adding nanotitanium dioxide and quaternary ammonium salt hyperbranched polyester to PVC materials, it improves its antibacterial and mechanical properties, and solves the problems of microbial breeding and health hazards during use of PVC materials, achieving significant improvements in antibacterial and mechanical properties.

CN118931068AInactive Publication Date: 2024-11-12JIEYANG ZHENGXIN SHOES IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411262173.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing PVC materials are prone to contamination and breeding of microorganisms during use, leading to health hazards, and lack of antibacterial properties, making it difficult to effectively solve this problem.

Method used

Antibacterial PVC materials composed of PVC, plasticizer, calcium-zinc stabilizer, nanotitanium dioxide modified PVC and quaternary ammonium salt hyperbranched polyester are prepared through high-speed mixing, double-roll refining and flat plate vulcanization processes to increase nanotitanium dioxide The compatibility and antibacterial activity of quaternary ammonium salts improve the antibacterial and mechanical properties of the material.

Benefits of technology

The prepared antibacterial PVC material has significantly improved antibacterial properties and mechanical properties, which can effectively inhibit the growth of microorganisms and improve the tolerance to external shocks, and significantly improve the tensile strength and impact strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931068A_ABST
    Figure CN118931068A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of PVC, and discloses an antibacterial PVC material and a preparation method thereof.The antibacterial PVC material is obtained by adding quaternary ammonium salt-terminated hyperbranched polyester, nano titanium dioxide modified PVC and the like into PVC to be evenly mixed and tabletted. The prepared PVC material contains a quaternary ammonium salt structure and nano titanium dioxide, both the quaternary ammonium salt structure and the nano titanium dioxide are good antibacterial structures, and the antibacterial property of the PVC material can be improved when the quaternary ammonium salt structure and the nano titanium dioxide are applied to the PVC material. Besides, due to the fact that the quaternary ammonium salt-terminated hyperbranched polyester contains many branched chain structures, the quaternary ammonium salt-terminated hyperbranched polyester and the PVC material can form a chemically and physically cross-linked three-dimensional network structure, the mechanical property of the PVC material can be further improved, the contained nanometer titanium dioxide particles can also serve as stress concentration points to absorb much energy, and the mechanical property of the material is further improved. The PVC material prepared by the preparation method disclosed by the invention has relatively good antibacterial property and mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PVC, in particular to an antibacterial PVC material and a preparation method thereof. Background Art

[0002] Polyvinyl chloride (PVC) is one of the most widely used polymer materials today. It has excellent chemical stability, mechanical properties and other properties, and is widely used in various fields of life and work. Since PVC plastic products prepared from PVC are easily contaminated and breed a variety of microorganisms, including pathogenic bacteria, during use, which can cause harm to human health, it is of great practical significance to carry out antibacterial and sterilization treatment on PVC plastic products.

[0003] Nano-titanium dioxide has the characteristics of small particle size, high photocatalytic activity and ultraviolet absorption ability, and is widely used in sewage treatment, air purification, cosmetics, coatings and other fields. Quaternary ammonium salt antibacterial agent is a broad-spectrum antibacterial agent with strong antibacterial ability and strong penetration ability, and is widely used in various industries. Hyperbranched polymers have unique highly branched structures and multi-functional characteristics, and have a very broad application space.

[0004] For example, the patent with authorization announcement number CN 105218964 B discloses an antibacterial polyvinyl chloride material and its preparation method and application. The material includes polyvinyl chloride resin, a combined antibacterial agent, a plasticizer, etc. The prepared material has good antibacterial properties. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides an antibacterial PVC material and a preparation method thereof. The prepared PVC material has good antibacterial properties and mechanical properties.

[0007] (II) Technical solution

[0008] An antibacterial PVC material, the antibacterial PVC material is composed of the following components by weight: 100 parts by weight of PVC, 40-55 parts by weight of a plasticizer, 2-4 parts by weight of a calcium zinc stabilizer, 50-100 parts by weight of nano-titanium dioxide modified PVC, and 1-10 parts by weight of a quaternary ammonium salt hyperbranched polyester;

[0009] The preparation method of the antibacterial PVC material is:

[0010] PVC, plasticizer, calcium zinc stabilizer, nano titanium dioxide modified PVC, and terminal quaternary ammonium salt hyperbranched polyester are added into a high-speed mixer, fully mixed, placed on a double-roll mill for mixing, and then placed in a flat vulcanizer for tableting to obtain an antibacterial PVC material.

[0011] Preferably, the mixing temperature is 160° C. and the mixing time is 5 min.

[0012] Preferably, the parameters set for the flat-plate vulcanizer are: hot pressing at 180° C. and 10 MPa for 5 min, and cold pressing at 20° C. and 10 MPa for 5 min.

[0013] Preferably, the preparation method of the nano-titanium dioxide modified PVC is:

[0014] (1) Add nano-titanium dioxide to a flask filled with deionized water, disperse it with ultrasound, add a 10% hydrochloric acid aqueous solution to control the pH to 4-5, then add γ-methacryloxypropyltrimethoxysilane to it, react at 50-70° C. for 1-2 hours, centrifuge after the reaction, wash with deionized water, and dry to obtain olefinated nano-titanium dioxide;

[0015] (2) Under nitrogen conditions, PVC and benzoyl peroxide are added to a flask containing 1,2-dichloroethane solvent, stirred and dispersed, and then olefinated nano-titanium dioxide is added thereto. The reaction is carried out at 70-80°C for 3-6 hours. After the reaction is completed, methanol is added thereto, filtered, washed with deionized water, and dried to obtain nano-titanium dioxide modified PVC.

[0016] Preferably, in (1), the amount of γ-methacryloxypropyltrimethoxysilane used is 0.5-1% of the mass of the nano-titanium dioxide.

[0017] Preferably, in (2), the amount of benzoyl peroxide used is 3-5% of the mass of PVC; the amount of olefinated nano-titanium dioxide used is 20-40% of the mass of PVC.

[0018] Preferably, the preparation method of the terminal quaternary ammonium salt hyperbranched polyester is:

[0019] S1. Under nitrogen conditions, pentaerythritol and 2,2-dimethylolpropionic acid are added to a flask, stirred and dispersed, and p-toluenesulfonic acid is added thereto at 130-140° C., melted for 2-4 hours, and then vacuumed for 2-5 hours. After the reaction is completed, the temperature is lowered to 45-55° C., dissolved in acetone, precipitated with n-hexane, and dried to obtain a hyperbranched polyester;

[0020] S2. Under nitrogen conditions, add the hyperbranched polyester into a flask filled with N,N-dimethylformamide solvent, stir and disperse, add sodium hydroxide and epichlorohydrin, react at 45-55°C for 20-48h, after the reaction is completed, remove the solid by vacuum filtration, add octadecyl dimethyl tertiary amine, react at 50-60°C for 10-24h, after the reaction is completed, rotary evaporate and dry to obtain terminal quaternary ammonium salt hyperbranched polyester.

[0021] Preferably, in S1, the mass ratio of pentaerythritol to 2,2-dimethylolpropionic acid is 1:12-15; and the amount of p-toluenesulfonic acid used is 1-4% of the total mass of pentaerythritol and 2,2-dimethylolpropionic acid.

[0022] Preferably, in S2, the mass ratio of the hyperbranched polyester, sodium hydroxide, epichlorohydrin and octadecyldimethyl tertiary amine is 1:0.01-0.02:0.45-0.6:1.4-1.8.

[0023] (III) Beneficial technical effects

[0024] The invention uses PVC as a raw material and olefinated nano titanium dioxide as a grafting monomer, and under the initiation of benzoyl peroxide, nano titanium dioxide is grafted to the PVC side chain to prepare nano titanium dioxide modified PVC. Pentaerythritol is used as a core and 2,2-dihydroxymethyl propionic acid is used as a growth monomer. Under the catalysis of p-toluenesulfonic acid, hyperbranched polyester is synthesized, and the polyester is used as a raw material to sequentially react with epichlorohydrin and octadecyl dimethyl tertiary amine through etherification reaction and quaternization reaction to obtain terminal quaternary ammonium salt hyperbranched polyester, and finally the polyester and nano titanium dioxide modified PVC are added to PVC, mixed evenly, and tableted to obtain an antibacterial PVC material.

[0025] The antibacterial PVC material prepared by the present invention contains nano titanium dioxide particles and quaternary ammonium salt structure, and the nano titanium dioxide has good photocatalytic antibacterial effect, but because it has high surface energy, it is very easy to reunite, therefore, the present invention is grafted into the PVC material, increases its compatibility with the PVC material, and then improves its antibacterial effect in the PVC material. The quaternary ammonium salt with positive charge can be adsorbed to the surface of microbial cells with negative charge by electrostatic attraction, combines with the phospholipid bilayer in the cytoplasmic membrane, destroys the cytoplasmic membrane, causes the release of intracellular substances, and causes cell death. Both nano titanium dioxides have good antibacterial properties, and are applied to the PVC material to improve the antibacterial properties of the PVC material.

[0026] The terminal quaternary ammonium salt hyperbranched polyester prepared by the present invention has a large amount of ester groups in its molecule interior, the carbonyl oxygen in this group can interact with the methine hydrogen atom on the PVC segment to form a hydrogen bond, forming chemical crosslinking, because the terminal quaternary ammonium salt hyperbranched polyester contains more branched structures, it can form a physical crosslinking effect with the PVC molecular chain, just because there is chemical crosslinking and physical crosslinking, both have good compatibility and form more crosslinking sites, when the PVC material is subjected to external impact, external energy can be dispersed on other molecular chains and consumed by a large number of crosslinking sites, thereby improving the mechanical properties of the PVC material. In addition, because it contains nano titanium dioxide inorganic particles, it can be used as a stress concentration point, absorbs more external energy, and further improves the mechanical properties of the PVC material. The PVC material prepared by the present invention has good antibacterial properties and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a reaction synthesis route for hyperbranched polyester;

[0028] Figure 2 This is the infrared spectrum of hyperbranched polyester. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] (1) 10 g of nano titanium dioxide was added to a flask filled with deionized water, and ultrasonically dispersed. A 10% hydrochloric acid aqueous solution was added thereto to control the pH to 5, and then 0.05 g of γ-methacryloxypropyltrimethoxysilane was added thereto. The mixture was reacted at 70° C. for 2 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain olefinated nano titanium dioxide.

[0032] (2) Under nitrogen conditions, 20 g of PVC and 0.8 g of benzoyl peroxide were added to a flask filled with 1,2-dichloroethane solvent, stirred and dispersed, and then 5 g of olefinated nano-titanium dioxide was added thereto. The reaction was carried out at 75° C. for 5 h. After the reaction was completed, methanol was added thereto, the mixture was filtered, washed with deionized water, and dried to obtain nano-titanium dioxide modified PVC.

[0033] (3) Under nitrogen conditions, 5 g of pentaerythritol and 70 g of 2,2-dimethylolpropionic acid were added to a flask, stirred and dispersed, and 1 g of p-toluenesulfonic acid was added thereto at 140° C., melt-reacted for 4 h, and then vacuum-reacted for 2 h. After the reaction was completed, the temperature was lowered to 50° C., dissolved in acetone, precipitated with n-hexane, and dried to obtain a hyperbranched polyester.

[0034] (4) Under nitrogen conditions, 20 g of the hyperbranched polyester was added to a flask filled with N,N-dimethylformamide solvent, and the mixture was stirred and dispersed. 0.4 g of sodium hydroxide and 10 g of epichlorohydrin were added thereto, and the mixture was reacted at 50° C. for 20 h. After the reaction was completed, the solid was removed by vacuum filtration. 30 g of octadecyldimethyl tertiary amine was added thereto, and the mixture was reacted at 50° C. for 24 h. After the reaction was completed, the mixture was rotary evaporated and dried to obtain a terminal quaternary ammonium salt hyperbranched polyester.

[0035] (5) 100 g of PVC, 55 g of dioctyl phthalate plasticizer, 2 g of calcium zinc stabilizer, 50 g of nano-titanium dioxide modified PVC, and 1 g of terminal quaternary ammonium salt hyperbranched polyester were added to a high-speed mixer and mixed thoroughly. The mixture was placed on a double-roll mill for mixing at a mixing temperature of 160° C. for 5 min. The mixture was then placed in a flat-plate vulcanizer for sheeting. The parameters set for the flat-plate vulcanizer were: hot pressing at 180° C. and 10 MPa for 5 min, and cold pressing at 20° C. and 10 MPa for 5 min, to obtain an antibacterial PVC material.

[0036] Example 2

[0037] (1) 10 g of nano titanium dioxide was added to a flask filled with deionized water, and ultrasonically dispersed. A 10% hydrochloric acid aqueous solution was added thereto to control the pH to 4, and then 0.1 g of γ-methacryloxypropyltrimethoxysilane was added thereto. The mixture was reacted at 50° C. for 2 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain olefinated nano titanium dioxide.

[0038] (2) Under nitrogen conditions, 20 g of PVC and 0.8 g of benzoyl peroxide were added to a flask filled with 1,2-dichloroethane solvent, stirred and dispersed, and then 5 g of olefinated nano-titanium dioxide was added thereto. The reaction was carried out at 75° C. for 6 h. After the reaction was completed, methanol was added thereto, the mixture was filtered, washed with deionized water, and dried to obtain nano-titanium dioxide modified PVC.

[0039] (3) Under nitrogen conditions, 5 g of pentaerythritol and 65 g of 2,2-dimethylolpropionic acid were added to a flask, stirred and dispersed, and 2 g of p-toluenesulfonic acid was added thereto at 140° C., melt-reacted for 4 h, and then vacuum-reacted for 3 h. After the reaction was completed, the temperature was lowered to 50° C., dissolved in acetone, precipitated with n-hexane, and dried to obtain a hyperbranched polyester.

[0040] (4) Under nitrogen conditions, 20 g of hyperbranched polyester was added to a flask filled with N,N-dimethylformamide solvent, stirred and dispersed, 0.2 g of sodium hydroxide and 9 g of epichlorohydrin were added thereto, and the reaction was carried out at 55° C. for 48 h. After the reaction was completed, the solid was removed by vacuum filtration, and 28 g of octadecyldimethyl tertiary amine was added thereto, and the reaction was carried out at 60° C. for 10 h. After the reaction was completed, the mixture was rotary evaporated and dried to obtain a terminal quaternary ammonium salt hyperbranched polyester.

[0041] (5) 100 g of PVC, 45 g of dioctyl phthalate plasticizer, 4 g of calcium zinc stabilizer, 60 g of nano-titanium dioxide modified PVC, and 3 g of terminal quaternary ammonium salt hyperbranched polyester were added to a high-speed mixer and mixed thoroughly. The mixture was placed on a double-roll mill for mixing at a mixing temperature of 160° C. for 5 min. The mixture was then placed in a flat-plate vulcanizer for sheeting. The parameters set for the flat-plate vulcanizer were: hot pressing at 180° C. and 10 MPa for 5 min, and cold pressing at 20° C. and 10 MPa for 5 min, to obtain an antibacterial PVC material.

[0042] Example 3

[0043] (1) 10 g of nano titanium dioxide was added to a flask filled with deionized water, and ultrasonically dispersed. A 10% hydrochloric acid aqueous solution was added thereto to control the pH to 4, and then 0.08 g of γ-methacryloxypropyltrimethoxysilane was added thereto. The mixture was reacted at 60° C. for 1 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain olefinated nano titanium dioxide.

[0044] (2) Under nitrogen conditions, 20 g of PVC and 0.6 g of benzoyl peroxide were added to a flask filled with 1,2-dichloroethane solvent, stirred and dispersed, and then 5 g of olefinated nano-titanium dioxide was added thereto. The reaction was carried out at 80° C. for 4 h. After the reaction was completed, methanol was added thereto, the mixture was filtered, washed with deionized water, and dried to obtain nano-titanium dioxide modified PVC.

[0045] (3) Under nitrogen conditions, 5 g of pentaerythritol and 60 g of 2,2-dimethylolpropionic acid were added to a flask, stirred and dispersed, and 0.65 g of p-toluenesulfonic acid was added thereto at 135° C., melt-reacted for 2 h, and then vacuum-reacted for 4 h. After the reaction was completed, the temperature was lowered to 50° C., dissolved in acetone, precipitated with n-hexane, and dried to obtain a hyperbranched polyester.

[0046] (4) Under nitrogen conditions, 20 g of the hyperbranched polyester was added to a flask filled with N,N-dimethylformamide solvent, and the mixture was stirred and dispersed. 0.3 g of sodium hydroxide and 12 g of epichlorohydrin were added thereto, and the mixture was reacted at 45° C. for 24 h. After the reaction was completed, the solid was removed by vacuum filtration. 36 g of octadecyldimethyl tertiary amine was added thereto, and the mixture was reacted at 55° C. for 12 h. After the reaction was completed, the mixture was rotary evaporated and dried to obtain a terminal quaternary ammonium salt hyperbranched polyester.

[0047] (5) 100 g of PVC, 40 g of dioctyl phthalate plasticizer, 4 g of calcium zinc stabilizer, 70 g of nano-titanium dioxide modified PVC, and 5 g of terminal quaternary ammonium salt hyperbranched polyester were added to a high-speed mixer and mixed thoroughly. The mixture was placed on a double-roll mill for mixing at a mixing temperature of 160° C. for 5 min. The mixture was then placed in a flat-plate vulcanizer for sheeting. The parameters set for the flat-plate vulcanizer were as follows: hot pressing at 180° C. and 10 MPa for 5 min, and cold pressing at 20° C. and 10 MPa for 5 min, to obtain an antibacterial PVC material.

[0048] Example 4

[0049] (1) 10 g of nano titanium dioxide was added to a flask filled with deionized water, and ultrasonically dispersed. A 10% hydrochloric acid aqueous solution was added thereto to control the pH to 5, and then 0.06 g of γ-methacryloxypropyltrimethoxysilane was added thereto. The mixture was reacted at 55° C. for 2 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain olefinated nano titanium dioxide.

[0050] (2) Under nitrogen conditions, 20 g of PVC and 0.8 g of benzoyl peroxide were added to a flask filled with 1,2-dichloroethane solvent, stirred and dispersed, and then 8 g of olefinated nano-titanium dioxide was added thereto. The reaction was carried out at 70° C. for 6 h. After the reaction was completed, methanol was added thereto, the mixture was filtered, washed with deionized water, and dried to obtain nano-titanium dioxide modified PVC.

[0051] (3) Under nitrogen conditions, 5 g of pentaerythritol and 75 g of 2,2-dimethylolpropionic acid were added to a flask, stirred and dispersed, and 3.2 g of p-toluenesulfonic acid was added thereto at 130° C., melt-reacted for 4 h, and then vacuum-reacted for 2 h. After the reaction was completed, the temperature was lowered to 45° C., dissolved in acetone, precipitated with n-hexane, and dried to obtain a hyperbranched polyester.

[0052] (4) Under nitrogen conditions, 20 g of the hyperbranched polyester was added to a flask filled with N,N-dimethylformamide solvent, and the mixture was stirred and dispersed. 0.3 g of sodium hydroxide and 10 g of epichlorohydrin were added thereto, and the mixture was reacted at 55° C. for 24 h. After the reaction was completed, the solid was removed by vacuum filtration. 36 g of octadecyldimethyl tertiary amine was added thereto, and the mixture was reacted at 55° C. for 24 h. After the reaction was completed, the mixture was rotary evaporated and dried to obtain a terminal quaternary ammonium salt hyperbranched polyester.

[0053] (5) 100 g of PVC, 50 g of dioctyl phthalate plasticizer, 3 g of calcium zinc stabilizer, 80 g of nano-titanium dioxide modified PVC, and 8 g of terminal quaternary ammonium salt hyperbranched polyester were added to a high-speed mixer and mixed thoroughly. The mixture was placed on a double-roll mill for mixing at a mixing temperature of 160° C. for 5 min. The mixture was then placed in a flat-plate vulcanizer for sheeting. The parameters set for the flat-plate vulcanizer were as follows: hot pressing at 180° C. and 10 MPa for 5 min, and cold pressing at 20° C. and 10 MPa for 5 min, to obtain an antibacterial PVC material.

[0054] Example 5

[0055] (1) 10 g of nano titanium dioxide was added to a flask filled with deionized water, and ultrasonically dispersed. A 10% hydrochloric acid aqueous solution was added thereto to control the pH to 4, and then 0.1 g of γ-methacryloxypropyltrimethoxysilane was added thereto. The mixture was reacted at 60° C. for 2 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain olefinated nano titanium dioxide.

[0056] (2) Under nitrogen conditions, 20 g of PVC and 1 g of benzoyl peroxide were added to a flask filled with 1,2-dichloroethane solvent, stirred and dispersed, and then 4 g of olefinated nano-titanium dioxide was added thereto. The reaction was carried out at 75°C for 3 h. After the reaction was completed, methanol was added thereto, the mixture was filtered, washed with deionized water, and dried to obtain nano-titanium dioxide modified PVC.

[0057] (3) Under nitrogen conditions, 5 g of pentaerythritol and 65 g of 2,2-dimethylolpropionic acid were added to a flask, stirred and dispersed, and 2 g of p-toluenesulfonic acid was added thereto at 140° C., melt-reacted for 3 h, and then vacuum-reacted for 5 h. After the reaction was completed, the temperature was lowered to 55° C., dissolved in acetone, precipitated with n-hexane, and dried to obtain a hyperbranched polyester.

[0058] (4) Under nitrogen conditions, 20 g of the hyperbranched polyester was added to a flask filled with N,N-dimethylformamide solvent, stirred and dispersed, 0.4 g of sodium hydroxide and 11 g of epichlorohydrin were added thereto, and the reaction was carried out at 50° C. for 48 h. After the reaction was completed, the solid was removed by vacuum filtration, and 32 g of octadecyldimethyl tertiary amine was added thereto, and the reaction was carried out at 60° C. for 16 h. After the reaction was completed, the mixture was rotary evaporated and dried to obtain a terminal quaternary ammonium salt hyperbranched polyester.

[0059] (5) 100 g of PVC, 50 g of dioctyl phthalate plasticizer, 4 g of calcium zinc stabilizer, 100 g of nano-titanium dioxide modified PVC, and 10 g of terminal quaternary ammonium salt hyperbranched polyester were added to a high-speed mixer and mixed thoroughly. The mixture was placed on a double-roll mill for mixing at a mixing temperature of 160° C. for 5 min. The mixture was then placed in a flat-plate vulcanizer for sheeting. The parameters set for the flat-plate vulcanizer were as follows: hot pressing at 180° C. and 10 MPa for 5 min, and cold pressing at 20° C. and 10 MPa for 5 min, to obtain an antibacterial PVC material.

[0060] Comparative Example 1

[0061] The difference between this comparative example and Example 1 is that in step (5), no nano-titanium dioxide-modified PVC is contained.

[0062] Comparative Example 2

[0063] The difference between this comparative example and Example 1 is that in step (5), no terminal quaternary ammonium salt hyperbranched polyester is contained.

[0064] Use an electronic universal testing machine to test the tensile properties of PVC materials.

[0065] Use an impact tester to test the impact performance of PVC materials.

[0066] Table 1: Mechanical properties test results of various embodiments and comparative examples

[0067]

[0068]

[0069] As can be seen from the table, the PVC material prepared by the present invention has good mechanical properties, the maximum tensile strength can reach 24.17MPa, and the maximum impact strength can reach 41.09kg·m -2 .

[0070] The PVC material was cut into 2 cm × 2 cm sheets, the surface was wiped with alcohol and sterilized under UV light, the bacterial strain and culture medium were mixed at a ratio of 1:1000, and cultured in a shaker at 37 °C until the bacterial concentration reached 6-8 × 107 CFU / mL, and dilute it to 5×10 5 CFU / mL, 32 μL of bacterial solution was added on the PVC sheet, covered with a coverslip, and placed in a bacterial incubator for 24 h, then 4 mL of phosphate buffer solution was added thereto, covered with a coverslip, and placed in a shaker at 37°C for 30 min, the phosphate buffer solution containing bacteria was diluted with phosphate buffer solution at a ratio of 1:100, placed on a plate spreader for plating, and then placed in an incubator at 37°C for 24 h, the culture medium with colonies was photographed and counted under a colony counter, antibacterial rate (%) = (the number of colonies in the blank control group - the number of colonies in the antibacterial sample) / the number of colonies in the blank control group × 100%, and the test bacteria were Escherichia coli and Staphylococcus aureus.

[0071] Table 2: Antibacterial performance test results of various embodiments and comparative examples

[0072]

[0073]

[0074] It can be seen from the table that the antibacterial PVC material prepared by the present invention has good antibacterial performance, and the antibacterial performance against Escherichia coli and Staphylococcus aureus can reach up to 99.9%. This is because the quaternary ammonium salt groups and nano titanium dioxide particles contained therein work synergistically to improve the antibacterial performance of the PVC material.

[0075] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and modifications made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the scope of protection of the present invention.

Claims

1. An antibacterial PVC material, characterized in that: The antibacterial PVC material is composed of the following components by weight: 100 parts by weight of PVC, 40-55 parts by weight of a plasticizer, 2-4 parts by weight of a calcium zinc stabilizer, 50-100 parts by weight of nano-titanium dioxide modified PVC, and 1-10 parts by weight of a quaternary ammonium salt hyperbranched polyester; The preparation method of the antibacterial PVC material is: PVC, plasticizer, calcium zinc stabilizer, nano titanium dioxide modified PVC, and terminal quaternary ammonium salt hyperbranched polyester are added into a high-speed mixer, fully mixed, placed on a double-roll mill for mixing, and then placed in a flat vulcanizer for tableting to obtain an antibacterial PVC material.

2. The antibacterial PVC material according to claim 1, characterized in that: The mixing temperature is 160° C. and the mixing time is 5 min.

3. The antibacterial PVC material according to claim 1, characterized in that: The parameters set for the flat plate vulcanizer are: hot pressing at 180°C and 10 MPa for 5 min, and cold pressing at 20°C and 10 MPa for 5 min.

4. The antibacterial PVC material according to claim 1, characterized in that: The preparation method of the nano titanium dioxide modified PVC is: (1) Add nano-titanium dioxide to a flask filled with deionized water, disperse it with ultrasound, add a 10% hydrochloric acid aqueous solution to control the pH to 4-5, then add γ-methacryloxypropyltrimethoxysilane to it, react at 50-70° C. for 1-2 hours, centrifuge after the reaction, wash with deionized water, and dry to obtain olefinated nano-titanium dioxide; (2) Under nitrogen conditions, PVC and benzoyl peroxide are added to a flask containing 1,2-dichloroethane solvent, stirred and dispersed, and then olefinated nano-titanium dioxide is added thereto. The reaction is carried out at 70-80°C for 3-6 hours. After the reaction is completed, methanol is added thereto, filtered, washed with deionized water, and dried to obtain nano-titanium dioxide modified PVC.

5. The antibacterial PVC material according to claim 4, characterized in that: In the above (1), the amount of γ-methacryloxypropyltrimethoxysilane used is 0.5-1% of the mass of nano-titanium dioxide.

6. The antibacterial PVC material according to claim 4, characterized in that: In the above (2), the amount of benzoyl peroxide used is 3-5% of the mass of PVC; the amount of olefinated nano titanium dioxide used is 20-40% of the mass of PVC.

7. The antibacterial PVC material according to claim 1, characterized in that: The preparation method of the terminal quaternary ammonium salt hyperbranched polyester is: S1. Under nitrogen conditions, pentaerythritol and 2,2-dimethylolpropionic acid are added to a flask, stirred and dispersed, and p-toluenesulfonic acid is added thereto at 130-140° C., melted for 2-4 hours, and then vacuumed for 2-5 hours. After the reaction is completed, the temperature is lowered to 45-55° C., dissolved in acetone, precipitated with n-hexane, and dried to obtain a hyperbranched polyester; S2. Under nitrogen conditions, add the hyperbranched polyester into a flask filled with N,N-dimethylformamide solvent, stir and disperse, add sodium hydroxide and epichlorohydrin, react at 45-55°C for 20-48h, after the reaction is completed, remove the solid by vacuum filtration, add octadecyl dimethyl tertiary amine, react at 50-60°C for 10-24h, after the reaction is completed, rotary evaporate and dry to obtain terminal quaternary ammonium salt hyperbranched polyester.

8. The antibacterial PVC material according to claim 7, characterized in that: In the S1, the mass ratio of pentaerythritol to 2,2-dimethylolpropionic acid is 1:12-15; the amount of p-toluenesulfonic acid used is 1-4% of the total mass of pentaerythritol and 2,2-dimethylolpropionic acid.

9. The antibacterial PVC material according to claim 7, characterized in that: In S2, the mass ratio of the hyperbranched polyester, sodium hydroxide, epichlorohydrin and octadecyldimethyl tertiary amine is 1:0.01-0.02:0.45-0.6:1.4-1.8.

Citation Information

Patent Citations

  • Modified polyvinyl chloride resin powder coating

    CN103396708A

  • Organosilicon-modified PVC composite material

    CN106380763A