Preparation method of master batch with high wear resistance and high temperature resistance

Through enrichment and segmented calcining technology, the content of quartz in coal gangue is reduced and its wear resistance and high temperature resistance is improved. The problems of high quartz content and poor wear resistance in the existing technology are solved, and the coal gangue is realized. High value is applied in the field of rubber and plastic materials.

CN118931088APending Publication Date: 2024-11-12ZHENGZHOU MINERALS COMPOSITIVE UTILIZATION RES INST CHINESE GEOLOGICAL ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979541.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art has failed to effectively reduce the quartz content in coal gangue, limiting its application scope, and has not improved the wear resistance and high temperature resistance of coal gangue.

Method used

Coal gangue powder with low quartz content is prepared by enrichment and reducing miscellaneous materials, and the wear resistance and high temperature resistance are improved through segmented calcination and addition of specific additives, including pretreatment crushing, fluidized bed airflow grinding, screening, and division. calcination and the use of additives.

Benefits of technology

The high wear resistance and high temperature resistance of coal gangue has been achieved, which has improved its comprehensive utilization value, reduced production costs, and made the prepared masterbatches widely used in the field of rubber and plastic materials, which has improved the wear resistance of rubber and plastic materials and High temperature resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of coal gangue resource utilization, and relates to a preparation method of a high-wear-resistance and high-temperature-resistance master batch. Comprising the following steps: 1, enriching and reducing impurities to prepare coal gangue powder with low quartz content; 2, calcining to prepare a powder filler; and 3, preparing the master batch with high wear resistance and high temperature resistance. The comprehensive utilization value of the coal gangue is improved; the prepared master batch has high wear resistance and high temperature resistance; the technological process is simple and the production cost is low; through segmented calcination and additive addition, effective utilization of quartz and clay in coal gangue is realized. The prepared master batch can be widely applied to the field of rubber and plastic materials, and the wear resistance and high temperature resistance of the rubber and plastic materials are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coal gangue resource utilization and relates to a method for preparing a highly wear-resistant and high-temperature resistant masterbatch. Background Art

[0002] In some areas, the proportion of quartz in the mineral composition of coal gangue is relatively high, usually greater than 50%, and the other components are mainly clay (greater than 20%), which is mainly used for low-end products such as brick making and road construction. Due to the high proportion of quartz in the composition and the low clay content, the scope of application is limited. After reducing the proportion of quartz, coal gangue can be used as filler for rubber and plastic materials.

[0003] In the existing technology, some related patent technologies are disclosed, for example: the invention patent application with application publication number CN113956682A discloses a rubber reinforcing filler and a method for preparing a rubber reinforcing filler by using activated modified coal gangue. The method comprises the following steps: providing coal gangue raw materials; crushing the coal gangue raw materials; ultrafine grinding the crushed coal gangue raw materials to obtain coal gangue particles; airflow classification of the coal gangue particles to obtain coal gangue microparticles; activating the coal gangue microparticles; surface modifying and grinding the activated coal gangue microparticles to obtain modified coal gangue microparticles. However, the patent does not mention how to reduce the quartz content, nor how to improve wear resistance and high temperature resistance. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a highly wear-resistant and high-temperature resistant masterbatch, wherein low-quartz content coal gangue powder is prepared by enriching and reducing impurities, and the wear resistance and high-temperature resistance are improved by staged calcination and adding additives.

[0005] The present invention specifically includes the following technical solutions:

[0006] 1. Enrichment and reduction of impurities to prepare coal gangue powder with low quartz content:

[0007] Step 1. Pre-treat and crush the gangue, and the particle size after crushing is D50≤20mm; the quartz content in the gangue in this step is greater than 50wt%;

[0008] Step 2. Put the crushed coal gangue into a fluidized bed jet mill, add 0.2-5wt% of additive A, and perform a crushing operation by adjusting the classifying wheel. Product 1 is obtained at the discharge port, and product 2 is obtained in the dust removal bag; wherein additive A is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:1-2:1-2:0.5-3;

[0009] Step 3. Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3;

[0010] Step 4. After mixing product 2 and product 3, perform secondary crushing to obtain a powder with a D97 of 18 μm, namely product 4; the quartz content in the product 4 is 10-20wt%, and the silicate clay content is 80-90wt%.

[0011] 2. Calcination to prepare powder filler:

[0012] Step 5. Add 3-5wt% of additive B to product 4, where additive B is prepared by mixing sodium chloride, boric acid and magnesium sulfate in a mass ratio of 3-5:1-2.5:0.5-2. Perform staged calcination in a muffle furnace, rotary kiln or microwave calcination furnace, wherein the first stage is heated from room temperature to 350°C at a heating rate of 10°C / min and kept warm for 30 minutes; the second stage is heated to 750°C at a heating rate of 20°C / min and kept warm for 10 minutes; the third stage is heated to 850-900°C at a heating rate of 10°C / min and kept warm for 30 minutes, then quickly cooled to 300°C, cooled naturally at room temperature, and cooled to room temperature; the calcined powder is crushed to 800 mesh to obtain product 5, i.e., powder filler.

[0013] 3. Preparation of highly wear-resistant and high temperature resistant masterbatch:

[0014] Step 6. Prepare an additive C solution, add the additive C solution to product 5, stir and blend to obtain a filler; in the filler, the additive C solution accounts for 3-6wt%; the additive C is a mixture of a silane coupling agent, polydimethyldiallyl ammonium chloride, and carboxymethyl chitosan; during mixing, anhydrous ethanol is added to the additive C solution for dilution, and the mass ratio of the additive C solution to anhydrous ethanol is 1:1. In the process of adding the additive C solution to product 5 for extrusion and blending to prepare the filler, the anhydrous ethanol will volatilize. In the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallyl ammonium chloride, and carboxymethyl chitosan is 3-4:1-2:1-2.

[0015] Step 7. Put the mixed filler into a high-speed mixer and stir at 105°C for 1 hour; extrude and blend the filler at 60wt% and the matrix resin at 40wt% to prepare a gangue masterbatch. The matrix resin is PP-maleic anhydride (PP-g-MAH) or ABS.

[0016] The beneficial effects of the present invention include:

[0017] The invention improves the comprehensive utilization value of coal gangue; the prepared masterbatch has high wear resistance and high temperature resistance; the process flow is simple and the production cost is low; through staged calcination and adding additives, the quartz and clay in the coal gangue are effectively utilized; the prepared masterbatch can be widely used in the field of rubber and plastic materials to improve the wear resistance and high temperature resistance of rubber and plastic materials.

[0018] (1) The present invention uses low-value coal gangue with a quartz content greater than 50wt% as raw material to prepare high-value, highly wear-resistant and high-temperature-resistant masterbatch, converting low-value minerals into high-value products, significantly improving economic efficiency.

[0019] (2) The present invention can effectively reduce the impurity content by adding additives of specific composition when crushing coal gangue, and can also better separate quartz and silicate clay, thereby improving the separation efficiency. In addition, the quartz content is ensured to be maintained at 10wt%-20wt% by combining the screening of the particle size after multiple crushings, because the appropriate amount of quartz will change its phase after subsequent calcination, which can improve the wear resistance of the product.

[0020] (3) The present invention adds additives in a specific proportion when calcining the gangue powder in stages, wherein the purpose of the staged calcination is, first, to remove impurities and improve whiteness; second, to help regulate the crystal form, change the quartz structure, and improve wear resistance. The first stage of calcination removes organic matter, the second stage of calcination removes iron, and the third stage of calcination causes the silicon-aluminum ratio to change in the physical phase structure under specific temperature, insulation time, and quenching conditions to form a special structure, which is beneficial for preparing powders and improving the wear resistance and high temperature resistance of later products. The addition of additives can synergistically improve its high temperature resistance and changes in the crystal structure, which is beneficial for phase reconstruction and improves overall wear resistance and high temperature resistance. DETAILED DESCRIPTION

[0021] The present invention is described in more detail below through specific implementation modes to facilitate understanding of the technical solution of the present invention, but is not intended to limit the protection scope of the present invention.

[0022] Embodiment 1:

[0023] Coal gangue from a certain area was selected, with a quartz content of 55wt% and a clay content of 30wt%.

[0024] 1. Enrichment and reduction of impurities to prepare coal gangue powder with low quartz content:

[0025] Step 1. Pre-treat and crush the gangue to a particle size of D50≤20mm after crushing;

[0026] Step 2. Put the crushed coal gangue into a fluidized bed jet mill, add 0.2wt% of additive A, and perform a crushing operation by adjusting the classifying wheel. Product 1 is obtained at the discharge port, and product 2 is obtained in the dust removal bag; wherein additive A is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:1:1:0.5;

[0027] Step 3. Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3;

[0028] Step 4. Mix product 2 and product 3 and grind them twice to obtain a powder with a D97 of 18 μm, i.e., product 4;

[0029] 2. Calcination to prepare powder filler:

[0030] Step 5. Add 3wt% of additive B to product 4, where additive B is mixed with sodium chloride, boric acid and magnesium sulfate in a mass ratio of 3:1:0.5; calcine in stages through a muffle furnace, a rotary kiln or a microwave calcining furnace, heating to 350°C in the first stage, heating rate of 10°C / min, and keeping warm for 30 minutes; heating to 750°C in the second stage, heating rate of 20°C / min, and keeping warm for 10 minutes; heating to 850°C in the third stage, heating rate of 10°C / min, and keeping warm for 30 minutes, then quickly cooling to 300°C, cooling naturally at room temperature, and cooling to room temperature; crushing the calcined powder to 800 mesh to obtain product 5, i.e., powder filler. The whiteness of the powder after calcination is 90.

[0031] 3. Preparation of highly wear-resistant and high temperature resistant masterbatch:

[0032] Step 6. Prepare an additive C solution, add it to product 5, stir and blend to obtain a filler; in the filler, the additive C solution accounts for 3wt%; the additive C solution is a mixture of a silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan; in the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallylammonium chloride, and carboxymethyl chitosan is 3:1:2; anhydrous ethanol is also added to the additive C solution during mixing, and the mass ratio of the additive C solution to anhydrous ethanol is 1:1.

[0033] Step 7. Put the mixed filler into a high-speed mixer and stir at 105°C for 1 hour; extrusion blend the filler at 60wt% and the matrix resin at 40wt% to prepare a coal gangue masterbatch. The matrix resin is PP-maleic anhydride (PP-g-MAH).

[0034] Example 2

[0035] Coal gangue from a certain area was selected, with a quartz content of 50wt% and a clay content of 25wt%.

[0036] 1. Enrichment and reduction of impurities to prepare coal gangue powder with low quartz content:

[0037] Step 1. Pre-treat and crush the gangue to a particle size of D50≤30mm after crushing;

[0038] Step 2. Put the crushed coal gangue into a fluidized bed jet mill, add 5wt% of additive A, and perform a crushing operation by adjusting the classifying wheel. Product 1 is obtained at the discharge port, and product 2 is obtained in the dust removal bag; wherein additive A is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:2:2:3;

[0039] Step 3. Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3;

[0040] Step 4. Mix product 2 and product 3 and grind them twice to obtain a powder with a D97 of 18 μm, i.e., product 4;

[0041] 2. Calcination process for preparing powder filler:

[0042] Step 5. Add 5wt% of additive B to product 4, where additive B is a mixture of sodium chloride, boric acid and magnesium sulfate in a mass ratio of 5:2.5:0.2; calcine in stages using a muffle furnace, a rotary kiln or a microwave calcining furnace, wherein the first stage is heated to 350°C at a heating rate of 10°C / min and kept warm for 30 minutes; the second stage is heated to 750°C at a heating rate of 20°C / min and kept warm for 10 minutes; the third stage is heated to 900°C at a heating rate of 10°C / min and kept warm for 30 minutes, then quickly cooled to 300°C, cooled naturally at room temperature, and cooled to room temperature; the calcined powder is crushed to 800 meshes to obtain product 5, i.e., powder filler. The whiteness of the calcined powder is 92.

[0043] 3. Preparation of high wear-resistant and high temperature resistant masterbatch:

[0044] Step 6. Prepare an additive C solution, add it to product 5, stir and blend, and obtain a filler; in the filler, the additive C solution accounts for 3wt%; the additive C solution is a mixture of a silane coupling agent, polydimethyldiallyl ammonium chloride, and carboxymethyl chitosan; during mixing, anhydrous ethanol is added to the additive C solution for dilution, and the mass ratio of the additive C solution to anhydrous ethanol is 1:1. In the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallyl ammonium chloride, and carboxymethyl chitosan is 4:2:2.

[0045] Step 7. Put the mixed filler into a high-speed mixer and stir at 105°C for 1 hour; extrusion blend the filler at 60wt% and the matrix resin at 40wt% to prepare a coal gangue masterbatch. The matrix resin is PP-maleic anhydride (PP-g-MAH).

[0046] Comparative Example 1

[0047] The difference from Example 1 is that the composition of additive A during pulverization is ammonium chloride and sodium oleate, and the mass ratio of the two is 3:2.

[0048] Comparative Example 2

[0049] The difference from Example 1 is that during calcination, additive B is a mixture of sodium chloride and boric acid in a mass ratio of 3:1.

[0050] Comparative Example 3

[0051] The difference from Example 1 is that during calcination, the temperature is directly raised to 850°C at a heating rate of 10°C / min, kept at that temperature for 30 minutes, then quickly cooled to 300°C, and naturally cooled to room temperature at room temperature.

[0052] Comparative Example 4

[0053] The difference from Example 1 is that after calcination, the mixture is air-cooled instead of being rapidly cooled to 300° C., but is directly cooled naturally to room temperature at room temperature.

[0054] Dynamic friction coefficient Thermal deformation temperature / ℃ Tensile strength / Mpa <![CDATA[Quartz content (SiO2%)]]> Example 1 0.24 135 45 15.3 Example 2 0.25 135 43 16.8 Comparative Example 1 0.45 132 37 38.5 Comparative Example 2 0.32 123 36 15.7 Comparative Example 3 0.29 125 38 15.8 Comparative Example 4 0.34 130 35 15.5

[0055] The above description is only a detailed description of the present invention in combination with a specific preferred embodiment, but the present invention is not limited thereto. Without departing from the concept of the present invention, if it still falls within the technical scope, the technical solution of the present invention can be subjected to a variety of simple modifications such as several simple deductions or replacements, including the combination of various technical features in any other appropriate manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a highly wear-resistant and high-temperature resistant masterbatch, characterized in that: The following steps are involved: Step 1. Pre-treat and crush the gangue to a particle size of D50≤20mm after crushing; Step 2. Add 0.2-5wt% of additive A to the crushed coal gangue, grind it with a jet mill, obtain product 1 at the discharge port, and obtain product 2 in the dust removal bag; Step 3. Screen product 1, discard the particles larger than 50 μm, and the particles below the screen are product 3; Step 4. Mix product 2 and product 3 and grind them twice to obtain a powder with a D97 of 18 μm, i.e., product 4; Step 5. Add 3-5 wt% of additive B to product 4, perform segmented calcination, and finally crush to 800 mesh to obtain product 5; Step 6. Add the additive C solution to the product 5, stir and blend, and obtain a filler; the additive C solution accounts for 3-6wt% of the filler; The additive C solution is prepared by mixing a silane coupling agent, polydimethyldiallyl ammonium chloride and carboxymethyl chitosan; in the additive C solution, the mass ratio of the silane coupling agent, polydimethyldiallyl ammonium chloride and carboxymethyl chitosan is 3-4:1-2:1-2; Step 7: Extrude and blend the filler obtained in step 6 at a ratio of 60 wt% of filler and 40 wt% of matrix resin to prepare coal gangue masterbatch.

2. The method according to claim 1, characterized in that The quartz content in the coal gangue of step 1 is greater than 50wt%.

3. The method according to claim 1, characterized in that The additive A described in step 2 is prepared by mixing ammonium chloride, sodium oleate, triethanolamine and dodecyltrimethylammonium chloride in a mass ratio of 3:1-2:1-2:0.5-3.

4. The method according to claim 1, characterized in that The additive B described in step 5 is prepared by mixing sodium chloride, boric acid and magnesium sulfate in a mass ratio of 3-5:1-2.5:0.5-2.

5. The method according to claim 1, characterized in that The staged calcination parameters described in step 5 are: the first stage is heated from room temperature to 350°C, the heating rate is 10°C / min, and the temperature is kept for 30 minutes; the second stage is heated to 750°C, the heating rate is 20°C / min, and the temperature is kept for 10 minutes; the third stage is heated to 850-900°C, the heating rate is 10°C / min, and the temperature is kept for 30 minutes, and quenched to 300°C, and then naturally cooled to room temperature.

6. The method according to claim 1, characterized in that The product 4 has a quartz content of 10-20 wt % and a silicate clay content of 80-90 wt %.

7. The method according to claim 1, characterized in that In step 6, anhydrous ethanol is also added to the additive C solution during mixing, and the mass ratio of the additive C solution to anhydrous ethanol is 1:

1.

8. The method according to claim 1, characterized in that In step 7, the filler mixed in step 6 is first stirred at 105° C. for 1 hour, and then the mixed filler and the matrix resin are extruded and blended.

9. The method according to claim 1, characterized in that In step 7, the base resin is PP-maleic anhydride or ABS.