High-viscosity PET composite material and preparation method thereof

By adding antibacterial agents and chain extenders to PET composite materials and granulating them with twin screw extruders, the problem of insufficient viscosity and antibacterial performance in the automotive materials field is solved, and efficient PET composites are achieved Material preparation expands its application range.

CN118931129AInactive Publication Date: 2024-11-12赵光辉
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411241175.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing PET composite materials cannot meet the requirements of high viscosity and antibacterial properties in the field of automotive materials, limiting their application scope.

Method used

The preparation method of high viscosity PET composite materials includes mixing PET, antibacterial agent, chain extender diethyltoluenediamine and antioxidant in a specific proportion, and granulating through a twin screw extruder to prepare an improved antibacterial Performance PET composite material.

Benefits of technology

It improves the antibacterial properties and viscosity of PET composites and expands its application range in the material field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029326130000011
    Figure BDA0005029326130000011
  • Figure BDA0005029326130000111
    Figure BDA0005029326130000111
Patent Text Reader

Abstract

The invention belongs to the field of PET composite materials, and particularly relates to a high-viscosity PET composite material and a preparation method thereof, and the high-viscosity PET composite material comprises the following raw materials by weight: 80-100 parts of PET; 0.4 to 0.6 part of diethyltoluenediamine serving as a chain extender; 2-4 parts of an antibacterial agent; the preparation method comprises the following steps: S1, weighing 80 to 100 parts of PET, 2 to 4 parts of an antibacterial agent, 0.4 to 0.6 part of a chain extender diethyltoluenediamine and 0.1 to 0.5 part of an antioxidant, mixing, and uniformly stirring, so as to obtain a mixture. The antibacterial PET material has the advantages of good antibacterial performance and viscosity; the material can be used in the fields of materials such as spray bottles of products such as cosmetics, medicines and living disinfection articles, and has an excellent application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of PET composite materials, and in particular to a high-viscosity PET composite material and a preparation method thereof. Background Art

[0002] Polyethylene terephthalate (PET) is a widely used polymer polyester resin. PET has the advantages of good fatigue resistance, good heat resistance, excellent dimensional stability, etc. However, in some specific automotive material fields, high requirements are placed on the viscosity and antibacterial properties of PET. Ordinary PET materials can no longer meet these requirements, which limits the application of PET composite materials in some material fields. Summary of the invention

[0003] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high-viscosity PET composite material and a preparation method thereof.

[0004] The high-viscosity PET composite material proposed by the present invention comprises the following raw materials in parts by weight:

[0005]

[0006] A method for preparing a high-viscosity PET composite material comprises the following steps:

[0007] S1, weigh 80-100 parts of PET, 2-4 parts of antibacterial agent, 0.4-0.6 parts of chain extender diethyltoluenediamine, and 0.1-0.5 parts of antioxidant, mix and stir evenly to obtain a mixture;

[0008] S2, extruding the mixed material obtained in S1 through a twin-screw extruder to form pellets, thereby obtaining a PET composite material.

[0009] Preferably, the twin-screw extruder includes six temperature zones arranged in sequence, with the temperature of zone one at 240-260°C, the temperature of zone two at 280-300°C, the temperature of zone three at 280-300°C, the temperature of zone four at 280-300°C, the temperature of zone five at 280-300°C, the temperature of zone six at 280-300°C, the head temperature at 280-300°C, and the screw speed at 200-280r / min.

[0010] Preferably, the method for preparing the antibacterial agent comprises the following steps:

[0011] (1) Weigh a certain amount of copper acetate, potassium bicarbonate, and deionized water, add them to a reaction vessel, and stir the reaction at 40-60° C. for 8-12 hours to obtain solution A;

[0012] (2) Filtering solution A, washing, drying in a vacuum drying oven at 60-70° C. for 6-10 hours, cooling and grinding through an 800-mesh sieve to obtain copper oxide;

[0013] (3) Weigh a certain amount of copper oxide, salicylaldehyde, isocyanate propyl triethoxysilane, catalyst benzoyl peroxide, acetone, and deionized water, add them to a reaction vessel, react at 50-70° C. for 6-8 hours, filter, wash, and place in a vacuum drying oven at 50-70° C. for 8 hours to 12 hours to obtain a salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type antibacterial agent.

[0014] Preferably, the mass ratio of the copper acetate, potassium bicarbonate and deionized water is (20-30):(40-50):(70-90).

[0015] Preferably, the mass ratio of the copper oxide, salicylaldehyde, isocyanatepropyltriethoxysilane, catalyst dibutyltin dilaurate, acetone, and deionized water is (30-36): (20-30): (16-20): (0.5-0.7): (60-70): (90-100).

[0016] Preferably, the antioxidant is one or a mixture of tris(2,4-di-tert-butyl)phenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.

[0017] Preferably, the temperature of the vacuum drying oven is detected, and the detected temperature is compared with the preset temperature. When the temperature reaches the preset temperature, the staff is reminded to filter and wash solution A, dry it at 60-70°C in a vacuum drying oven for 6-10h, cool it, grind it through an 800-mesh sieve to obtain copper oxide.

[0018] Preferably, in S3, a certain amount of copper oxide, salicylaldehyde, isocyanate propyl triethoxysilane, catalyst benzoyl peroxide, acetone, and deionized water are weighed and added to a reaction vessel, and reacted at 50-70° C. for 6-8 hours. The reaction temperature is monitored, and when the temperature is not within the range of 50-70° C., an early warning is issued and the temperature is controlled by a thermostat.

[0019] Preferably, a certain amount of copper acetate, potassium bicarbonate and deionized water are weighed, added to a reaction vessel, stirred and reacted at 40-60° C. for 8-12 hours to obtain solution A, and the reaction temperature is monitored. When the temperature is not within the range of 40-60° C., an early warning is issued and the temperature is controlled by a thermostat.

[0020] The principle of antimicrobial synthesis is as follows:

[0021] Mg(CH3COO)2+2KHCO3→2CH3COOK+Mg(HCO3)2

[0022] Mg(HCO3)2→MgO+2CO2+H2O.

[0023] The beneficial effects of the present invention are:

[0024] The invention synthesizes a novel salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type antibacterial agent. On the one hand, isocyanate propyl triethoxysilane is hydrolyzed to generate Si-OH, and Si-OH undergoes a dehydration condensation reaction to form siloxane, which is coated on the surface of MgO. On the other hand, isocyanate of isocyanate propyl triethoxysilane can undergo a Cookes reaction with the aldehyde group of salicylaldehyde to generate products such as alkyl urea and pseudo-aldehyde isocyanate, thereby finally forming a salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type antibacterial agent.

[0025] The invention synthesizes a novel salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type antibacterial agent, which can well improve the antibacterial property of PET composite material.

[0026] The addition of chain extender diethyltoluenediamine can increase the molecular weight of PET, thereby increasing the viscosity of PET composites. DETAILED DESCRIPTION

[0027] The present invention will be further explained below in conjunction with specific embodiments.

[0028] The raw materials used in the following examples are as follows:

[0029] PET (model 008L), Ac lo, Canada; copper acetate, Shandong Xinghai Chemical Co., Ltd.; potassium bicarbonate, Shandong Poly Chemical Co., Ltd.; salicylaldehyde, Hubei Chengfeng Chemical Co., Ltd.; deionized water, Xiamen Aoquan Environmental Protection Technology Co., Ltd.; isocyanate propyl triethoxysilane, Guangzhou Shanghe Chemical Technology Co., Ltd.; benzoyl peroxide, Jinan Shuangying Chemical Co., Ltd.; acetone, Shandong Changyuan Chemical Co., Ltd.; chain extender diethyltoluenediamine, Shandong Poly Chemical Co., Ltd.; titanium dioxide, Hebei Bangti Chemical Co., Ltd.; antioxidants (Irganox168, Irganox1010, Irganox1330), BASF, Germany.

[0030] Preparation Example 1

[0031] (1) Weigh 200 g of copper acetate, 400 g of potassium bicarbonate, and 700 g of deionized water, add them into a reaction vessel, and stir at 40° C. for 8 h to obtain solution A.

[0032] (2) Filter solution A, wash it, dry it in a vacuum drying oven at 60-70° C. for 6-10 hours, cool it, grind it through a 800-mesh sieve, and obtain copper oxide.

[0033] (3) Weigh a certain amount of copper oxide, salicylaldehyde, isocyanate propyl triethoxysilane, catalyst benzoyl peroxide, acetone, and deionized water, add them to a reaction vessel, react at 50-70°C for 6-8 hours, filter, wash, and place in a vacuum drying oven at 50-70°C for 8h-12h to obtain a salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type antibacterial agent M1.

[0034] Example 1

[0035] (1) Weigh 90 parts of PET, 2 parts of mesoporous cerium oxide type antibacterial agent M1, 0.4 parts of chain extender diethyltoluenediamine, and 0.1 parts of Irganox1010, mix and stir evenly to obtain a mixture;

[0036] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material P1.

[0037] The twin-screw extruder comprises six temperature zones arranged in sequence, with the temperature of zone one at 240°C, the temperature of zone two at 280°C, the temperature of zone three at 280°C, the temperature of zone four at 280°C, the temperature of zone five at 280°C, the temperature of zone six at 280°C, the head temperature at 280°C, and the screw speed at 200r / min.

[0038] Preparation Example 2

[0039] (1) Weigh 300 g of copper acetate, 500 g of potassium bicarbonate, and 900 g of deionized water, add them into a reaction vessel, and stir at 60° C. for 12 h to obtain solution A.

[0040] (2) Solution A was filtered, washed, and dried in a vacuum drying oven at 70° C. for 10 h. The solution was cooled and ground to pass through an 800-mesh sieve to obtain copper oxide.

[0041] (3) Weigh 360 g of copper oxide, 300 g of salicylaldehyde, 200 g of isocyanate propyl triethoxysilane, 7 g of catalyst benzoyl peroxide, 700 g of acetone, and 1.0 kg of deionized water, add them to a reaction vessel, react at 70° C. for 8 h, filter, wash, and place in a vacuum drying oven at 70° C. for 12 h to obtain an antibacterial agent M2 of the salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type.

[0042] Example 2

[0043] (1) Weigh 110 parts of PET, 4 parts of antibacterial agent M2, 0.6 parts of chain extender diethyltoluenediamine, 0.1 parts of antioxidant Irganox 1010, and 0.4 parts of Irganox 168, mix and stir to obtain a mixture;

[0044] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material P2.

[0045] The twin-screw extruder includes six temperature zones arranged in sequence, with the temperature of zone one at 260°C, the temperature of zone two at 300°C, the temperature of zone three at 300°C, the temperature of zone four at 300°C, the temperature of zone five at 300°C, the temperature of zone six at 300°C, the head temperature at 300°C, and the screw speed at 280r / min.

[0046] Preparation Example 3

[0047] (1) Weigh 250 g of copper acetate, 450 g of potassium bicarbonate, and 800 g of deionized water, add them into a reaction vessel, and stir at 50° C. for 10 h to obtain solution A.

[0048] (2) Solution A was filtered, washed, and dried in a vacuum drying oven at 65° C. for 8 h. The solution was cooled and ground to pass through a 800-mesh sieve to obtain copper oxide.

[0049] (3) Weigh 330 g of copper oxide, 250 g of salicylaldehyde, 180 g of isocyanate propyl triethoxysilane, 6 g of catalyst benzoyl peroxide, 650 g of acetone, and 950 g of deionized water, add them to a reaction vessel, react at 60° C. for 7 h, filter, wash, and place in a vacuum drying oven at 60° C. for 10 h to obtain an antibacterial agent M3 of the salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type.

[0050] Example 3

[0051] (1) Weigh 100 parts of PET, 3 parts of antibacterial agent M3, 0.5 parts of chain extender diethyltoluenediamine, 0.1 parts of antioxidant Irganox 1010, and 0.2 parts of Irganox 168, mix and stir to obtain a mixture;

[0052] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material P3.

[0053] The twin-screw extruder includes six temperature zones arranged in sequence, with the temperature of zone one at 250°C, the temperature of zone two at 290°C, the temperature of zone three at 290°C, the temperature of zone four at 290°C, the temperature of zone five at 290°C, the temperature of zone six at 290°C, the head temperature at 290°C, and the screw speed at 240r / min.

[0054] Preparation Example 4

[0055] (1) Weigh 255 g of copper acetate, 435 g of potassium bicarbonate, and 765 g of deionized water, add them to a reaction vessel, and stir at 58° C. for 11 h to obtain solution A.

[0056] (2) Solution A was filtered, washed, and dried in a vacuum drying oven at 68° C. for 9.5 h. The solution was cooled and ground to pass through a 800-mesh sieve to obtain copper oxide.

[0057] (3) Weigh 355 g of copper oxide, 295 g of salicylaldehyde, 195 g of isocyanate propyl triethoxysilane, 6.5 g of catalyst benzoyl peroxide, 685 g of acetone, and 955 g of deionized water, add them to a reaction vessel, react at 69.5° C. for 7.5 h, filter, wash, and place in a vacuum drying oven at 59° C. for 11 h to obtain an antibacterial agent M4 of the salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type.

[0058] Example 4

[0059] (1) Weigh 97.5 parts of PET, 3.5 parts of antibacterial agent M4, 0.45 parts of chain extender diethyltoluenediamine, 0.1 parts of antioxidant Irganox 1010, and 0.1 parts of antioxidant Irganox 168, mix and stir to obtain a mixture;

[0060] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material P4.

[0061] The twin-screw extruder includes six temperature zones arranged in sequence, with the temperature of zone one at 255°C, the temperature of zone two at 298°C, the temperature of zone three at 298°C, the temperature of zone four at 298°C, the temperature of zone five at 298°C, the temperature of zone six at 298°C, the head temperature at 288°C, and the screw speed at 275r / min.

[0062] Preparation Example 5

[0063] (1) Weigh 205 g of copper acetate, 405 g of potassium bicarbonate, and 715 g of deionized water, add them to a reaction vessel, and stir the mixture at 49.5° C. for 10.5 h to obtain solution A.

[0064] (2) Solution A was filtered, washed, and dried in a vacuum drying oven at 63.5° C. for 9.5 h. The solution was cooled and ground to pass through a 800-mesh sieve to obtain copper oxide.

[0065] (3) Weigh 345 g of copper oxide, 275 g of salicylaldehyde, 195 g of isocyanate propyl triethoxysilane, 5.5 g of catalyst benzoyl peroxide, 625 g of acetone, and 965 g of deionized water, add them to a reaction vessel, react at 69.5° C. for 7.5 h, filter, wash, and place in a vacuum drying oven at 68° C. for 11 h to obtain an antibacterial agent M5 of the salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type.

[0066] Example 5

[0067] (1) Weigh 96.5 parts of PET, 3.5 parts of antibacterial agent M5, 0.48 parts of chain extender diethyltoluenediamine, and 0.25 parts of antioxidant Irganox 1330, mix and stir to obtain a mixture;

[0068] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material P5.

[0069] The twin-screw extruder includes six temperature zones arranged in sequence, with zone one at 248°C, zone two at 287°C, zone three at 287°C, zone four at 287°C, zone five at 287°C, zone six at 287°C, die head temperature at 287°C, and screw speed at 245r / min.

[0070] Comparative Example 1

[0071] (1) Weigh 96.5 parts of PET and 0.25 parts of antioxidant Irganox 1330, mix and stir evenly to obtain a mixture;

[0072] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material D1.

[0073] The twin-screw extruder includes six temperature zones arranged in sequence, with zone one at 248°C, zone two at 287°C, zone three at 287°C, zone four at 287°C, zone five at 287°C, zone six at 287°C, die head temperature at 287°C, and screw speed at 245r / min.

[0074] Comparative Example 2

[0075] (1) Weigh 96.5 parts of PET, 3.5 parts of antibacterial agent titanium dioxide, and 0.25 parts of antioxidant Irganox 1330, mix and stir evenly to obtain a mixture;

[0076] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material D2.

[0077] The twin-screw extruder includes six temperature zones arranged in sequence, with zone one at 248°C, zone two at 287°C, zone three at 287°C, zone four at 287°C, zone five at 287°C, zone six at 287°C, die head temperature at 287°C, and screw speed at 245r / min.

[0078] Comparative Example 3

[0079] (1) Weigh 96.5 parts of PET, 0.48 parts of chain extender ADR-4370S, and 0.25 parts of antioxidant Irganox 1330, mix and stir evenly to obtain a mixture;

[0080] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PET composite material D3.

[0081] The twin-screw extruder includes six temperature zones arranged in sequence, with zone one at 248°C, zone two at 287°C, zone three at 287°C, zone four at 287°C, zone five at 287°C, zone six at 287°C, die head temperature at 287°C, and screw speed at 245r / min.

[0082] The PET composite materials prepared in the above examples 1-5 and comparative examples 1-3 were made into test strips by injection molding machine, and the test data are as follows:

[0083]

[0084] It can be seen from the above table that the antibacterial performance and viscosity of Examples 1-5 are better than those of Comparative Examples 1-3.

[0085] This indicates that the PET resin composite material prepared by the method provided by the present invention has good antibacterial properties and viscosity, and can expand the application field of the PET resin composite material.

[0086] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high-viscosity PET composite material, characterized in that: The invention comprises the following raw materials in parts by weight: PET 80-100 parts Chain extender diethyltoluenediamine 0.4-0.6 parts 2-4 parts of antibacterial agent Antioxidant 0.1 part -0.5 part 2. A method for preparing a high-viscosity PET composite material, characterized in that: The following steps are involved: S1, weigh 80-100 parts of PET, 2-4 parts of antibacterial agent, 0.4-0.6 parts of chain extender diethyltoluenediamine, and 0.1-0.5 parts of antioxidant, mix and stir evenly to obtain a mixture; S2, extruding the mixed material obtained in S1 through a twin-screw extruder to form pellets, thereby obtaining a PET composite material.

3. The method for preparing a high-viscosity PET composite material according to claim 2, characterized in that: The twin-screw extruder includes six temperature zones arranged in sequence, with the temperature of zone one being 240-260°C, the temperature of zone two being 280-300°C, the temperature of zone three being 280-300°C, the temperature of zone four being 280-300°C, the temperature of zone five being 280-300°C, the temperature of zone six being 280-300°C, the temperature of the die head being 280-300°C, and the screw speed being 200-280r / min.

4. The method for preparing a high-viscosity PET composite material according to claim 2, characterized in that: The preparation method of the antibacterial agent comprises the following steps: (1) Weigh a certain amount of copper acetate, potassium bicarbonate, and deionized water, add them to a reaction vessel, and stir the reaction at 40-60° C. for 8-12 hours to obtain solution A; (2) Filtering solution A, washing it, drying it in a vacuum drying oven at 60-70° C. for 6-10 hours, cooling it, grinding it through an 800-mesh sieve, and obtaining copper oxide; (3) Weigh a certain amount of copper oxide, salicylaldehyde, isocyanate propyl triethoxysilane, catalyst benzoyl peroxide, acetone, and deionized water, add them to a reaction vessel, react at 50-70° C. for 6-8 hours, filter, wash, and place in a vacuum drying oven at 50-70° C. for 8 hours to 12 hours to obtain a salicylaldehyde / isocyanate propyl triethoxysilane / copper oxide type antibacterial agent.

5. The method for preparing a high-viscosity PET composite material according to claim 4, characterized in that: The mass ratio of the copper acetate, potassium bicarbonate and deionized water is (20-30):(40-50):(70-90).

6. The method for preparing a high-viscosity PET composite material according to claim 4, characterized in that: The mass ratio of the copper oxide, salicylaldehyde, isocyanate propyl triethoxysilane, catalyst dibutyltin dilaurate, acetone and deionized water is (30-36): (20-30): (16-20): (0.5-0.7): (60-70): (90-100).

7. The method for preparing a high-viscosity PET composite material according to claim 2, characterized in that: The antioxidant is one of tris(2,4-di-tert-butyl)phenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene or a mixture of several thereof.

8. The method for preparing a high-viscosity PET composite material according to claim 4, characterized in that: The temperature of the vacuum drying oven is detected and compared with the preset temperature. When the temperature reaches the preset temperature, the staff is reminded to filter and wash solution A, dry it at 60-70°C in a vacuum drying oven for 6-10 hours, cool it, grind it through an 800-mesh sieve to obtain copper oxide.

9. The method for preparing a high-viscosity PET composite material according to claim 1, characterized in that: In the S3, a certain amount of copper oxide, salicylaldehyde, isocyanate propyl triethoxysilane, catalyst benzoyl peroxide, acetone, and deionized water are weighed and added to a reaction vessel, and reacted at 50-70° C. for 6-8 hours. The reaction temperature is monitored. When the temperature is not within the range of 50-70° C., an early warning is issued and the temperature is controlled by a thermostat.

10. The method for preparing a high-viscosity PET composite material according to claim 4, characterized in that: Weigh a certain amount of copper acetate, potassium bicarbonate, and deionized water, add them to a reaction vessel, stir and react at 40-60°C for 8-12 hours to obtain solution A, monitor the reaction temperature, and when the temperature is not within the range of 40-60°C, issue an early warning and control the temperature through a thermostat.