High-flame-retardant nylon composite material and preparation method thereof
By preparing a composite of silicon-modified phenolic resin and guanidine-modified β-cyclodextrin with nylon 66, a highly flame-retardant nylon material was formed, which solved the problem of insufficient flame retardancy of nylon materials and achieved the effect of high flame retardancy and good tensile strength.
Patent Information
- Application Number
- CN202411005897.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The insufficient flame retardant properties of existing nylon materials limit their application in the electronics and electrical fields.
By preparing a high flame-retardant nylon composite material consisting of silicon-modified phenolic resin, guanidine-modified β-cyclodextrin, and nylon 66, the flame-retardant properties and tensile strength of the material are improved by utilizing the protective layer formed by silicon when heated and the decomposition of guanidine groups to produce non-flammable gases and form a char layer to inhibit combustion.
It achieves high flame retardancy and good tensile strength, enhancing the application potential of nylon materials in the electronics and electrical fields.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a highly flame-retardant nylon composite material and a preparation method thereof. Background Art
[0002] Nylon is an engineering plastic widely used in various fields. With the development of the electronics, electrical and other industries, the performance requirements for nylon are becoming more and more stringent, but its flammable nature limits its development. For example, application No. 201510655143.0 announces a stretch-resistant and breakdown-resistant insulating material and a preparation method thereof. The preparation method comprises the following steps: first internal mixing, second internal mixing, refining with an open mixing mill, calendering with a calender, and cooling to obtain a stretch-resistant and breakdown-resistant insulating material. The prepared insulating material has a tensile strength of more than 50 MPa and a breakdown field strength of more than 38 KV / mm; however, its flame retardant properties are not improved. Summary of the invention
[0003] 1. Technical issues to be solved
[0004] In view of the deficiencies of the prior art, the present invention provides a highly flame-retardant nylon composite material and a preparation method thereof, which has good flame-retardant and tensile effects.
[0005] (II) Technical solution
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a highly flame-retardant nylon composite material, comprising the following components by weight: 5-12 parts by weight of silicon-modified phenolic resin, 6-10 parts by weight of guanidine-modified β-cyclodextrin, 65-80 parts by weight of nylon 66, and 1-3 parts by weight of antioxidant 1010.
[0007] Preferably, the preparation method of the silicon-modified phenolic resin is:
[0008] (1) adding allyl glycidyl ether, tetrahydrofuran and chloroplatinic acid to a reactor, activating at 40-60° C. for 30-40 min, then dropping 1,1,3,3-tetramethyldisiloxane for 50-60 min, continuing the reaction at 50-65° C. for 5-6 h, cooling to room temperature after the reaction, adding activated carbon adsorbent, ultrasonically shaking for 30-35 min, removing the catalyst chloroplatinic acid, filtering, and rotary evaporation to obtain epoxypropyl-terminated polymer arms;
[0009] (2) adding 7-15 parts by weight of β-cyclodextrin to a sodium hydroxide solution, stirring evenly, adding 10-16 parts by weight of a glycidyl-terminated polymer arm, ultrasonically shaking at 45-60° C. for 30-35 minutes, cooling to room temperature, adding 12-15% hydrochloric acid dropwise until neutral, washing and drying to obtain silicon-modified β-cyclodextrin;
[0010] (3) adding 4-chloro-3,5-dimethylphenol and silicon-modified β-cyclodextrin to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 75-90° C. for 8-12 hours, and then distilling under reduced pressure, filtering and drying to obtain phenol-based cyclodextrin;
[0011] (4) dissolving phenol in water, then adding phenol-based cyclodextrin, paraformaldehyde and dihydrated oxalic acid, reacting at 90-110° C. for 2-5 hours, and obtaining silicon-modified phenolic resin after the reaction.
[0012] Preferably, the mass ratio of allyl glycidyl ether, tetrahydrofuran, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane in (1) is 1:1.1-1.2:0.02-0.03:0.7-0.9.
[0013] Preferably, the mass fraction of the sodium hydroxide solution in (2) is 14-17%.
[0014] Preferably, the mass ratio of 4-chloro-3,5-dimethylphenol to silicon-modified β-cyclodextrin in (3) is 1.6-2.4:1.
[0015] Preferably, the mass ratio of phenol, phenol-based cyclodextrin, paraformaldehyde and oxalic acid dihydrate in (4) is 1:0.8-1:1.2-1.4:0.02-0.03.
[0016] Preferably, the preparation method of the guanidine-modified β-cyclodextrin is:
[0017] S1. Add 5-12 parts by weight of guanidine acetic acid to 15-25 parts by weight of thionyl chloride, stir evenly, react at 65-75 ° C for 10-14h, filter after the reaction, wash and dry to obtain an intermediate;
[0018] S2. Add 8-13 parts by weight of silicon-modified β-cyclodextrin and 12-16 parts by weight of the intermediate into N,N-dimethylformamide solvent, stir to dissolve, continue to add 1-2 parts by weight of triethylamine catalyst, react at 80-95°C for 7-14h, and then distill under reduced pressure, wash, and dry to obtain guanidine-modified β-cyclodextrin.
[0019] Preferably, the preparation method of the highly flame-retardant nylon composite material is: adding silicon-modified phenolic resin, guanidine-modified β-cyclodextrin, nylon 66, and antioxidant 1010 into a twin-screw extruder, with a blending temperature of 180-190°C and an extrusion temperature of 170-180°C to obtain a highly flame-retardant nylon composite material.
[0020] (III) Beneficial technical effects
[0021] The invention obtains a highly flame-retardant nylon composite material by adding silicon-modified phenolic resin, guanidine-modified beta-cyclodextrin, nylon 66 and antioxidant 1010 into a twin-screw extruder, blending and extruding.
[0022] The alkenyl group in allyl glycidyl ether and the silicon-hydrogen bond in 1,1,3,3-tetramethyldisiloxane are subjected to addition reaction, and epoxy groups are introduced at the same time, thereby obtaining epoxy-terminated polymer arms, which are further subjected to addition reaction with hydroxyl groups in β-cyclodextrin to generate new hydroxyl groups, thereby obtaining silicon-modified β-cyclodextrin, which is further subjected to reaction with chlorine in 4-chloro-3,5-dimethylphenol to introduce phenolic hydroxyl groups to obtain phenol-based cyclodextrin, and phenol, phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid are reacted to obtain silicon-modified phenolic resin; guanidineacetic acid and dichlorothionyl are reacted to introduce acyl chloride groups to obtain an intermediate, and the hydroxyl groups in the silicon-modified β-cyclodextrin are reacted with acyl chloride in the intermediate to introduce guanidine groups, thereby obtaining guanidine-modified β-cyclodextrin.
[0023] The silicon element in the present invention can form a protective layer on the surface of the material when heated, and at the same time promote the carbonization of the surface of the material, inhibit the combustion reaction, and achieve a flame retardant effect; the cyclodextrin group in the silicon-modified phenolic resin and the guanidine-modified β-cyclodextrin can promote the formation of a carbon layer on the surface of the material at high temperature, reduce the contact between the material and external oxygen, thereby achieving a flame retardant effect; the phenolic resin in the silicon-modified phenolic resin itself has a certain flame retardancy and can play a flame retardant effect; the guanidine group in the guanidine-modified β-cyclodextrin has a certain smoke suppression effect, and can decompose to produce non-combustible gases such as nitrogen and ammonia during combustion, thereby achieving a flame retardant effect, and together constitute a flame retardant system.
[0024] During the co-extrusion process, the molecular chains of silicon-modified phenolic resin, guanidine-modified β-cyclodextrin and nylon 66 will be entangled to form a network of interpenetration. In addition, silicon-modified phenolic resin and guanidine-modified β-cyclodextrin have some identical chain segments, which increases their compatibility, makes the flame retardant system more evenly distributed, and improves its tensile strength. DETAILED DESCRIPTION
[0025] Example 1
[0026] (1) adding allyl glycidyl ether, tetrahydrofuran and chloroplatinic acid into a reactor, activating at 40° C. for 30 minutes, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, tetrahydrofuran, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:1.1:0.02:0.7, the dropping time is 50 minutes, and the reaction is continued at 50° C. for 5 hours. After the reaction is completed, the reaction is cooled to room temperature, an activated carbon adsorbent is added, ultrasonically vibrated for 30 minutes, the catalyst chloroplatinic acid is removed, filtered, and rotary evaporated to obtain a glycidyl-terminated polymer arm;
[0027] (2) adding 7 parts by weight of β-cyclodextrin to a 14% sodium hydroxide solution, stirring evenly, adding 10 parts by weight of epoxypropyl-terminated polymer arms, ultrasonically shaking at 45° C. for 30 min, cooling to room temperature, adding 12% hydrochloric acid dropwise until neutral, washing and drying to obtain silicon-modified β-cyclodextrin;
[0028] (3) adding 4-chloro-3,5-dimethylphenol and silicon-modified β-cyclodextrin to N,N-dimethylformamide solvent, wherein the mass ratio of 4-chloro-3,5-dimethylphenol to silicon-modified β-cyclodextrin is 1.6:1, stirring to dissolve, reacting at 75° C. for 8 h, and then distilling under reduced pressure, filtering and drying to obtain phenol-based cyclodextrin;
[0029] (4) dissolving phenol in water, and then adding phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid, wherein the mass ratio of phenol, phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid is 1:0.8:1.2:0.02, reacting at 90° C. for 2 h, and obtaining a silicon-modified phenolic resin after the reaction;
[0030] (5) adding 5 parts by weight of guanidine acetic acid to 15 parts by weight of thionyl chloride, stirring evenly, reacting at 65° C. for 10 h, filtering after the reaction, washing and drying to obtain an intermediate;
[0031] (6) Add 8 parts by weight of silicon-modified β-cyclodextrin and 12 parts by weight of the intermediate into N,N-dimethylformamide solvent, stir and dissolve, continue to add 1 part by weight of triethylamine catalyst, react at 80° C. for 7 hours, and then distill under reduced pressure, wash, and dry to obtain guanidine-modified β-cyclodextrin;
[0032] (7) 5 parts by weight of silicon-modified phenolic resin, 6 parts by weight of guanidine-modified β-cyclodextrin, 65 parts by weight of nylon 66, and 1 part by weight of antioxidant 1010 are added to a twin-screw extruder at a blending temperature of 180° C. and an extrusion temperature of 170° C. to obtain a highly flame-retardant nylon composite material.
[0033] Example 2
[0034] (1) adding allyl glycidyl ether, tetrahydrofuran and chloroplatinic acid into a reactor, activating at 60° C. for 40 min, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, tetrahydrofuran, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:1.2:0.03:0.9, the dropping time is 60 min, and the reaction is continued at 65° C. for 6 h. After the reaction is completed, the reaction is cooled to room temperature, an activated carbon adsorbent is added, ultrasonically vibrated for 35 min, the catalyst chloroplatinic acid is removed, filtered and rotary evaporated to obtain a glycidyl-terminated polymer arm;
[0035] (2) adding 15 parts by weight of β-cyclodextrin to a 17% sodium hydroxide solution, stirring evenly, adding 16 parts by weight of epoxypropyl-terminated polymer arms, ultrasonically shaking at 60° C. for 35 min, cooling to room temperature, adding 15% hydrochloric acid dropwise until neutral, washing and drying to obtain silicon-modified β-cyclodextrin;
[0036] (3) adding 4-chloro-3,5-dimethylphenol and silicon-modified β-cyclodextrin to N,N-dimethylformamide solvent, wherein the mass ratio of 4-chloro-3,5-dimethylphenol to silicon-modified β-cyclodextrin is 2.4:1, stirring and dissolving, reacting at 90° C. for 12 h, and then distilling under reduced pressure, filtering and drying to obtain phenol-based cyclodextrin;
[0037] (4) dissolving phenol in water, and then adding phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid, wherein the mass ratio of phenol, phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid is 1:1:1.4:0.03, reacting at 110° C. for 5 hours, and obtaining a silicon-modified phenolic resin after the reaction;
[0038] (5) adding 12 parts by weight of guanidine acetic acid to 25 parts by weight of dichlorothionyl, stirring evenly, reacting at 75° C. for 14 h, filtering after the reaction, washing and drying to obtain an intermediate;
[0039] (6) Add 13 parts by weight of silicon-modified β-cyclodextrin and 16 parts by weight of the intermediate into N,N-dimethylformamide solvent, stir and dissolve, continue to add 2 parts by weight of triethylamine catalyst, react at 95° C. for 14 hours, and then distill under reduced pressure, wash, and dry to obtain guanidine-modified β-cyclodextrin;
[0040] (7) 12 parts by weight of silicon-modified phenolic resin, 10 parts by weight of guanidine-modified β-cyclodextrin, 80 parts by weight of nylon 66, and 3 parts by weight of antioxidant 1010 are added into a twin-screw extruder at a blending temperature of 190° C. and an extrusion temperature of 180° C. to obtain a highly flame-retardant nylon composite material.
[0041] Example 3
[0042] (1) adding allyl glycidyl ether, tetrahydrofuran and chloroplatinic acid into a reactor, activating at 50° C. for 35 minutes, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, tetrahydrofuran, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:1.15:0.025:0.8, the dropping time is 55 minutes, and the reaction is continued at 57.5° C. for 5.5 hours. After the reaction is completed, the reaction is cooled to room temperature, an activated carbon adsorbent is added, ultrasonic vibration is performed for 32.5 minutes, the catalyst chloroplatinic acid is removed, and the reaction is filtered and rotary evaporated to obtain a glycidyl-terminated polymer arm;
[0043] (2) adding 11 parts by weight of β-cyclodextrin to a 15.5% sodium hydroxide solution, stirring evenly, adding 13 parts by weight of epoxypropyl-terminated polymer arms, ultrasonically shaking at 52.5° C. for 32.5 min, cooling to room temperature, adding 13.5% hydrochloric acid dropwise to neutralize, washing and drying to obtain silicon-modified β-cyclodextrin;
[0044] (3) adding 4-chloro-3,5-dimethylphenol and silicon-modified β-cyclodextrin to N,N-dimethylformamide solvent, wherein the mass ratio of 4-chloro-3,5-dimethylphenol to silicon-modified β-cyclodextrin is 1.6-2.4:1, stirring to dissolve, reacting at 82.5° C. for 10 h, and then distilling under reduced pressure, filtering and drying to obtain phenol-based cyclodextrin;
[0045] (4) dissolving phenol in water, and then adding phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid, wherein the mass ratio of phenol, phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid is 1:0.9:1.3:0.025, reacting at 100° C. for 3.5 hours, and obtaining a silicon-modified phenolic resin after the reaction;
[0046] (5) adding 8.5 parts by weight of guanidine acetic acid to 20 parts by weight of dichlorothionyl, stirring evenly, reacting at 70° C. for 12 h, filtering after the reaction, washing and drying to obtain an intermediate;
[0047] (6) adding 10.5 parts by weight of silicon-modified β-cyclodextrin and 14 parts by weight of the intermediate to N,N-dimethylformamide solvent, stirring and dissolving, adding 1.5 parts by weight of triethylamine catalyst, reacting at 87.5° C. for 10.5 hours, and then distilling under reduced pressure, washing, and drying to obtain guanidine-modified β-cyclodextrin;
[0048] (7) 8.5 parts by weight of silicon-modified phenolic resin, 8 parts by weight of guanidine-modified β-cyclodextrin, 72.5 parts by weight of nylon 66, and 2 parts by weight of antioxidant 1010 were added into a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 175° C. to obtain a highly flame-retardant nylon composite material.
[0049] Comparative Example 1
[0050] (1) adding 8.5 parts by weight of guanidine acetic acid to 20 parts by weight of dichlorothionyl, stirring evenly, reacting at 70° C. for 12 h, filtering after the reaction, washing and drying to obtain an intermediate;
[0051] (2) adding 10.5 parts by weight of silicon-modified β-cyclodextrin and 14 parts by weight of the intermediate into N,N-dimethylformamide solvent, stirring and dissolving, adding 1.5 parts by weight of triethylamine catalyst, reacting at 87.5° C. for 10.5 hours, and then distilling under reduced pressure, washing, and drying to obtain guanidine-modified β-cyclodextrin;
[0052] (3) 8 parts by weight of guanidine-modified β-cyclodextrin, 72.5 parts by weight of nylon 66, and 2 parts by weight of antioxidant 1010 were added to a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 175° C. to obtain a highly flame-retardant nylon composite material.
[0053] Comparative Example 2
[0054] (1) adding allyl glycidyl ether, tetrahydrofuran and chloroplatinic acid into a reactor, activating at 50° C. for 35 minutes, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, tetrahydrofuran, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:1.15:0.025:0.8, the dropping time is 55 minutes, and the reaction is continued at 57.5° C. for 5.5 hours. After the reaction is completed, the reaction is cooled to room temperature, an activated carbon adsorbent is added, ultrasonic vibration is performed for 32.5 minutes, the catalyst chloroplatinic acid is removed, and the reaction is filtered and rotary evaporated to obtain a glycidyl-terminated polymer arm;
[0055] (2) adding 11 parts by weight of β-cyclodextrin to a 15.5% sodium hydroxide solution, stirring evenly, adding 13 parts by weight of epoxypropyl-terminated polymer arms, ultrasonically shaking at 52.5° C. for 32.5 min, cooling to room temperature, adding 13.5% hydrochloric acid dropwise to neutralize, washing and drying to obtain silicon-modified β-cyclodextrin;
[0056] (3) adding 4-chloro-3,5-dimethylphenol and silicon-modified β-cyclodextrin to N,N-dimethylformamide solvent, wherein the mass ratio of 4-chloro-3,5-dimethylphenol to silicon-modified β-cyclodextrin is 1.6-2.4:1, stirring to dissolve, reacting at 82.5° C. for 10 h, and then distilling under reduced pressure, filtering and drying to obtain phenol-based cyclodextrin;
[0057] (4) dissolving phenol in water, and then adding phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid, wherein the mass ratio of phenol, phenol-based cyclodextrin, polyformaldehyde and dihydrated oxalic acid is 1:0.9:1.3:0.025, reacting at 100° C. for 3.5 hours, and obtaining a silicon-modified phenolic resin after the reaction;
[0058] (5) 8.5 parts by weight of silicon-modified phenolic resin, 72.5 parts by weight of nylon 66, and 2 parts by weight of antioxidant 1010 were added into a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 175° C. to obtain a highly flame-retardant nylon composite material.
[0059] Use an oxygen index meter to test the limiting oxygen index of the material, and use a horizontal and vertical combustion instrument to test the combustion level of the material.
[0060] Table 1: Flame retardancy tests.
[0061] project Limiting oxygen index (%) Combustion level Example 1 30 V-0 Example 2 32 V-0 Example 3 31 V-0 Comparative Example 1 20 V-1 Comparative Example 2 21 V-1
[0062] It can be seen from Table 1 that Examples 1-3 of the present invention have better flame retardant effects than Comparative Examples 1-2.
[0063] Tensile performance test: refer to GB / T1040.2-2006 standard, prepare the sample with the specification of 180×10×3mm, and the tensile rate is 2mm / min.
[0064] Table 2: Tensile strength test.
[0065] project Tensile strength(Mpa) Example 1 71.6 Example 2 72.8 Example 3 71.9 Comparative Example 1 65.7 Comparative Example 2 66.1
[0066] It can be seen from Table 2 that Examples 1-3 of the present invention have better tensile strength than Comparative Examples 1-2.
[0067] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A highly flame-retardant nylon composite material, characterized in that: The invention comprises the following components by weight: 5-12 parts by weight of silicon-modified phenolic resin, 6-10 parts by weight of guanidine-modified beta-cyclodextrin, 65-80 parts by weight of nylon 66, and 1-3 parts by weight of antioxidant 1010.
2. The highly flame-retardant nylon composite material according to claim 1, characterized in that: The preparation method of the silicon-modified phenolic resin is as follows: (1) adding allyl glycidyl ether, tetrahydrofuran and chloroplatinic acid to a reactor, activating at 40-60° C. for 30-40 min, then dropping 1,1,3,3-tetramethyldisiloxane for 50-60 min, continuing the reaction at 50-65° C. for 5-6 h, cooling to room temperature after the reaction, adding activated carbon adsorbent, ultrasonically shaking for 30-35 min, removing the catalyst chloroplatinic acid, filtering, and rotary evaporation to obtain epoxypropyl-terminated polymer arms; (2) adding 7-15 parts by weight of β-cyclodextrin to a sodium hydroxide solution, stirring evenly, adding 10-16 parts by weight of a glycidyl-terminated polymer arm, ultrasonically shaking at 45-60° C. for 30-35 minutes, cooling to room temperature, adding 12-15% hydrochloric acid dropwise until neutral, washing and drying to obtain silicon-modified β-cyclodextrin; (3) adding 4-chloro-3,5-dimethylphenol and silicon-modified β-cyclodextrin to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 75-90° C. for 8-12 hours, and then distilling under reduced pressure, filtering and drying to obtain phenol-based cyclodextrin; (4) dissolving phenol in water, then adding phenol-based cyclodextrin, paraformaldehyde and dihydrated oxalic acid, reacting at 90-110° C. for 2-5 hours, and obtaining silicon-modified phenolic resin after the reaction.
3. The highly flame-retardant nylon composite material according to claim 2, characterized in that: The mass ratio of allyl glycidyl ether, tetrahydrofuran, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane in (1) is 1:1.1-1.2:0.02-0.03:0.7-0.
9.
4. The highly flame-retardant nylon composite material according to claim 2, characterized in that: The mass fraction of the sodium hydroxide solution in (2) is 14-17%.
5. The highly flame-retardant nylon composite material according to claim 2, characterized in that: The mass ratio of 4-chloro-3,5-dimethylphenol to silicon-modified β-cyclodextrin in (3) is 1.6-2.4:
1.
6. The highly flame-retardant nylon composite material according to claim 2, characterized in that: The mass ratio of phenol, phenol-based cyclodextrin, paraformaldehyde and oxalic acid dihydrate in (4) is 1:0.8-1:1.2-1.4:0.02-0.
03.
7. The highly flame-retardant nylon composite material according to claim 1, characterized in that: The preparation method of the guanidine-modified β-cyclodextrin is as follows: S1. Add 5-12 parts by weight of guanidine acetic acid to 15-25 parts by weight of thionyl chloride, stir evenly, react at 65-75 ° C for 10-14h, filter after the reaction, wash and dry to obtain an intermediate; S2. Add 8-13 parts by weight of silicon-modified β-cyclodextrin and 12-16 parts by weight of the intermediate into N,N-dimethylformamide solvent, stir to dissolve, continue to add 1-2 parts by weight of triethylamine catalyst, react at 80-95°C for 7-14h, and then distill under reduced pressure, wash, and dry to obtain guanidine-modified β-cyclodextrin.
8. A method for preparing a highly flame-retardant nylon composite material according to any one of claims 1 to 7, characterized in that: The preparation method of the high flame retardant nylon composite material is as follows: silicon-modified phenolic resin, guanidine-modified β-cyclodextrin, nylon 66 and antioxidant 1010 are added into a twin-screw extruder, the blending temperature is 180-190° C., the extrusion temperature is 170-180° C., and the high flame retardant nylon composite material is obtained.