Polyurethane precursor-nano silicate mineral compound asphalt and preparation method thereof

Through the composite technology of polyurethane precursor and nanosilicate minerals, a covalent crosslinking network is formed, which solves the emission and performance problems of asphalt flue gas, realizes the high-temperature stability and smoke suppression effect of asphalt, simplifies the preparation process, and has significant value of application.

CN118931216APending Publication Date: 2024-11-12TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411251543.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing asphalt materials produce a large amount of harmful flue gas during use, affecting the health of construction workers and shortening their service life. The existing governance technology cannot be effectively applied under unorganized emissions, and commonly used modifiers affect performance and the preparation process is complex.

Method used

Polyurethane precursor-nano silicate mineral compound asphalt is used to form a covalent cross-linking network through the layered structure of nanosilicate minerals and the chemical reaction of polyurethane precursor, adsorbing and inhibiting flue gas release, combining high-speed shearing and Preparation of heat treatment technology.

Benefits of technology

It significantly reduces the emission rate of asphalt flue gas, improves the high temperature stability and use performance of asphalt, has simple preparation technology, and has significant engineering application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931216A_ABST
    Figure CN118931216A_ABST
Patent Text Reader

Abstract

The invention relates to the field of compositions of asphalt materials, in particular to polyurethane precursor-nano silicate mineral compound asphalt and a preparation method thereof. The polyurethane precursor-nano silicate mineral compound asphalt comprises matrix asphalt, and is characterized by further comprising a polyurethane precursor and a nano silicate mineral, and the polyurethane precursor-nano silicate mineral compound asphalt is prepared from the following components in parts by mass: 100 parts of matrix asphalt, 1 to 5 parts of polyurethane precursor and 1 to 5 parts of nano silicate mineral. The invention relates to a preparation method of polyurethane precursor-nano silicate mineral compound asphalt. The preparation method is characterized by comprising the following steps: i, taking matrix asphalt; ii, adding nano silicate minerals; (iii) adding a polyurethane precursor; and iv, shearing. The flue gas is reduced, and the process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of asphalt material compositions, in particular to a polyurethane precursor-nano silicate mineral compound asphalt and a preparation method thereof. Background Art

[0002] Asphalt pavement is widely used around the world due to its excellent road performance, and the amount of asphalt used has also increased dramatically. Asphalt is mainly composed of high molecular hydrocarbons and is a mixture with extremely complex chemical composition. During use, it usually needs to be heated to above 140°C to make it a flowing liquid for mixing, transportation and paving. Under high temperature conditions, ordinary hot-mix asphalt will produce a large amount of asphalt fumes with irritating odor and harmful, mainly containing volatile organic compounds, sulfides, nitrogen oxides and other atmospheric pollutants. Among them, polycyclic aromatic hydrocarbons in volatile organic compounds will seriously endanger the health of construction workers. In addition, with the release of asphalt fumes, the performance of asphalt materials will gradually deteriorate, shortening the service life of asphalt.

[0003] At present, the technology for treating asphalt flue gas mainly involves its collection and centralized treatment. Typical methods include combustion, adsorption, condensation, etc., which are passive flue gas treatment technologies. However, this technology is mostly used for organized emission sources such as asphalt mixing plants, and cannot be used in the case of unorganized emissions such as paving.

[0004] Studies have found that the purpose of emission reduction can be achieved by adding modifiers to asphalt. However, most admixtures not only affect the performance of asphalt, but also have no significant smoke suppression effect, and the preparation process is complicated. Summary of the invention

[0005] In order to overcome the defects of the prior art and provide an asphalt material composition which reduces smoke emission and has a simple preparation process, the present invention discloses a polyurethane precursor-nano silicate mineral compound asphalt and a preparation method thereof.

[0006] The present invention achieves the purpose of the invention through the following technical solutions: A polyurethane precursor-nano silicate mineral composite asphalt, including a base asphalt, characterized in that it also includes a polyurethane precursor and a nano silicate mineral, and the mass fractions of each component are as follows: Base asphalt: 100, Polyurethane precursor: 1~5, Nanosilicate minerals: 1~5.

[0007] The polyurethane precursor-nano silicate mineral compound asphalt is characterized by: The polyurethane precursor is isophorone diisocyanate; Isophorone diisocyanate, also known as IPDI, has an average molecular weight of about 222 and is a colorless to yellow liquid. Its main functional group is isocyanate (-NCO), which can react with amines, water, alcohols, acids, and bases containing active hydrogen atoms. The nano-silicate mineral is selected from at least one of organically modified nano-montmorillonite, namely organic montmorillonite, and attapulgite, namely organic montmorillonite, referred to as OMMT, and attapulgite, referred to as ATT.

[0008] The organic modification of nano-montmorillonite can refer to the following steps: Weigh 3g of purified nano-montmorillonite, add 200ml of water to make a suspension, stir evenly, add 2mol / L HCl / NaOH solution dropwise to adjust the pH value to 1-11, and pour the suspension into a three-necked flask. At the same time, weigh CTAB not exceeding 80% of the weight of montmorillonite and dissolve it in 50ml of water, heat it slightly to make it completely dissolved, and then drop it into the three-necked flask dropwise, continue to heat to 30℃~90℃, stir at a constant temperature and high speed to react for 0.5hour~4hour, cool, filter, wash (use AgNO, solution to check whether the halogen ions are clean), dry, grind, pass through a 200-mesh sieve, and obtain the organically modified nano-montmorillonite product, which is bottled for use.

[0009] The method for preparing the polyurethane precursor-nano silicate mineral compound asphalt is characterized by comprising the following steps: i. In parts by mass, take 100 parts of base asphalt into a container and heat to a molten state; ii. Add 1 to 5 parts by mass of nano-silicate minerals to the molten matrix asphalt obtained in step i, and shear at a speed of 2000r / min~2500r / min for 20min~30min to form modified asphalt, to the surface of the modified asphalt and the edge of the container without obvious distribution of the modifier, and the surface of the modified asphalt remains flat; iii. Add 1 to 5 parts by mass of a polyurethane precursor to the modified asphalt obtained in step ii, stir until no bubbles are generated, and then use a high-speed shearing machine to shear at a speed of 2000r / min~2500r / min until the volume of the modified asphalt no longer expands; iv. When the volume of the modified asphalt stops expanding, the speed of the shearing machine is increased to 4000r / min~5000r / min and shearing is carried out for 45min~75min. After the shearing is completed, the modified asphalt is grown in an oven to keep it in a molten state for 2 hours to complete the preparation.

[0010] The invention discloses a polyurethane precursor-nano silicate mineral composite odorless and smoke-suppressing asphalt and a preparation method thereof, which can effectively reduce the emission of asphalt smoke while ensuring the use performance of asphalt, and has a simple preparation process and significant engineering application value.

[0011] The present invention adopts polyurethane precursor-nano silicate mineral composite modifier to modify the matrix asphalt. The nano silicate mineral presents nano layered structure and large specific surface area, and its own surface is negatively charged, which plays a vital role in adsorbing and inhibiting the release of asphalt smoke under high temperature conditions. When the polyurethane precursor is added to the asphalt, it reacts chemically with the polar hydroxyl or amino groups present in the asphalt and the nano silicate mineral, and the reaction leads to the formation of carbamate compounds, which makes the nano silicate mineral show stronger organicity on the one hand, and on the other hand, the reaction of the polyurethane precursor and the asphalt expands the interlayer spacing of the nano silicate mineral to form an intercalation structure, thereby ensuring the stable dispersion of the nano silicate mineral layer in the asphalt adhesive. In this process, the polyurethane precursor reacts with the polar small molecules in the asphalt and aggregates into macromolecules, so that the asphaltene and colloid content in the asphalt colloid system are increased, and the high temperature stability of the asphalt can be further improved. Through the above-mentioned transformation, a three-dimensional covalent cross-linked network is formed in the modified asphalt, which can effectively intercept volatile organic matter and help to comprehensively reduce smoke emissions.

[0012] The present invention has the following beneficial effects: 1. The present invention adopts polyurethane precursor-nano silicate mineral to carry out composite modification of asphalt, and utilizes its physical-chemical synergistic effect to effectively adsorb flue gas through the unique layered structure and large specific surface area of ​​nano silicate mineral. The chemical reaction between polyurethane precursor and nano silicate mineral / asphalt molecules and the formed molecular cross-linking network can further reduce flue gas emissions, and the inhibition rate can reach 44.67%.

[0013] 2. The prepared composite odorless and smoke-suppressing asphalt has good physical properties, and the preparation process is simple and low-cost, which is conducive to practical application and promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a diagram of asphalt fume coverage based on PTFE filter membrane in comparative example and Examples 3 and 4. DETAILED DESCRIPTION

[0015] The present invention is further described below by means of specific examples.

[0016] Example 1 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 6g, Attapulgite: 9g.

[0017] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is attapulgite. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, and attapulgite is added to the base asphalt. The base asphalt is sheared at a speed of 2500 r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt. Isophorone diisocyanate solution is added to the modified asphalt, and stirred with a glass rod until no bubbles are generated. The modified asphalt is sheared at a speed of 2500 r / min with a shearing machine until the volume of the modified asphalt no longer expands. The speed of the shearing machine is increased to 4500 r / min and sheared for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0018] Example 2 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 6g, Attapulgite: 8g.

[0019] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is attapulgite. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, and attapulgite is added to the base asphalt. The base asphalt is sheared at a speed of 2500 r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt. Isophorone diisocyanate solution is added to the modified asphalt, and stirred with a glass rod until no bubbles are generated. The modified asphalt is sheared at a speed of 2500 r / min with a shearing machine until the volume of the modified asphalt no longer expands. The speed of the shearing machine is increased to 4500 r / min and sheared for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0020] Example 3 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 9g, Attapulgite: 9g.

[0021] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is attapulgite. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, and attapulgite is added to the base asphalt. The base asphalt is sheared at a speed of 2500 r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt. Isophorone diisocyanate solution is added to the modified asphalt, and stirred with a glass rod until no bubbles are generated. The modified asphalt is sheared at a speed of 2500 r / min with a shearing machine until the volume of the modified asphalt no longer expands. The speed of the shearing machine is increased to 4500 r / min and sheared for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0022] Example 4 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 9g, Attapulgite: 12g.

[0023] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is attapulgite. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, and attapulgite is added to the base asphalt. The base asphalt is sheared at a speed of 2500 r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt. Isophorone diisocyanate solution is added to the modified asphalt, and stirred with a glass rod until no bubbles are generated. The modified asphalt is sheared at a speed of 2500 r / min with a shearing machine until the volume of the modified asphalt no longer expands. The speed of the shearing machine is increased to 4500 r / min and sheared for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0024] Example 5 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 6g, Organic montmorillonite: 9g.

[0025] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2500r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2500r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 4500r / min for shearing for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0026] Example 6 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 6g, Organic montmorillonite: 12g.

[0027] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2500r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2500r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 4500r / min for shearing for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0028] Example 7 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 9g, Organic montmorillonite: 9g.

[0029] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2500r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2500r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 4500r / min for shearing for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0030] Example 8 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 12g, Organic montmorillonite: 9g.

[0031] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2500r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2500r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 4500r / min for shearing for 60 minutes. After the shearing is completed, it is grown in an oven at 170°C for 2 hours to complete the preparation.

[0032] Example 9 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 3g, Attapulgite: 15g.

[0033] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is attapulgite. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, and attapulgite is added to the base asphalt. The base asphalt is sheared at a speed of 2000 r / min for 20 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt. Isophorone diisocyanate solution is added to the modified asphalt, and stirred with a glass rod until no bubbles are generated. The modified asphalt is sheared at a speed of 2000 r / min with a shearing machine until the volume of the modified asphalt no longer expands. The speed of the shearing machine is increased to 4000 r / min and sheared for 45 minutes. After the shearing is completed, it is grown in an oven for 2 hours to complete the preparation.

[0034] Example 10 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 100 parts, Isophorone diisocyanate: 1 part, Attapulgite: 5 parts.

[0035] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is attapulgite. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, and attapulgite is added to the base asphalt. The base asphalt is sheared at a speed of 2100 r / min for 21 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt. Isophorone diisocyanate solution is added to the modified asphalt, and stirred with a glass rod until no bubbles are generated. The modified asphalt is sheared at a speed of 2100 r / min with a shearing machine until the volume of the modified asphalt no longer expands. The speed of the shearing machine is increased to 4200 r / min and sheared for 50 minutes. After the shearing is completed, it is grown in an oven for 2 hours to complete the preparation.

[0036] Embodiment 11 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 6g, Attapulgite: 12g.

[0037] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is attapulgite. The preparation steps are as follows: The base asphalt was heated to 170°C to make it molten, attapulgite was added to the base asphalt, and sheared at 2200 r / min for 23 min with a shearing machine until the base asphalt liquid surface remained smooth to obtain modified asphalt, and then isophorone diisocyanate solution was added to the modified asphalt, and stirred with a glass rod until no bubbles were generated, and then sheared at 2200 r / min with a shearing machine until the volume of the modified asphalt no longer expanded, and the speed of the shearing machine was increased to 4300 r / min for shearing for 55 min. After the shearing was completed, it was grown in an oven for 2 hours to complete the preparation.

[0038] Example 12 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 9g, Organic montmorillonite: 9g.

[0039] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2300 r / min for 25 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2300 r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 4500 r / min for shearing for 60 minutes. After the shearing is completed, it is grown in an oven for 2 hours to complete the preparation.

[0040] Embodiment 13 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 12g, Organic montmorillonite: 6g.

[0041] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2400 r / min for 27 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2400 r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 4700 r / min for shearing for 65 minutes. After the shearing is completed, it is grown in an oven for 2 hours to complete the preparation.

[0042] Embodiment 14 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 3g, Organic montmorillonite: 3g.

[0043] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2500 r / min for 27 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2500 r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 4800 r / min for shearing for 70 minutes. After the shearing is completed, it is grown in an oven for 2 hours to complete the preparation.

[0044] Embodiment 15 Polyurethane precursor-nano silicate mineral compound asphalt, the components and mass fractions are as follows: Base asphalt: 300g, Isophorone diisocyanate: 3g, Organic montmorillonite: 3g.

[0045] In this embodiment, the base asphalt is produced by Maoming Branch of Sinopec, the polyurethane precursor is isophorone diisocyanate, and the nano-silicate mineral is organic montmorillonite produced by Zhejiang Fenghong New Materials Co., Ltd. The preparation steps are as follows: The base asphalt is heated to 170°C to make it molten, organic montmorillonite is added to the base asphalt, and sheared at 2500 r / min for 30 minutes with a shearing machine until the base asphalt liquid surface remains smooth to obtain modified asphalt, and then isophorone diisocyanate solution is added to the modified asphalt, stirred with a glass rod until no bubbles are generated, and then sheared at 2500 r / min with a shearing machine until the volume of the modified asphalt no longer expands, and the shearing machine speed is increased to 5000 r / min for shearing for 75 minutes. After the shearing is completed, it is grown in an oven for 2 hours to complete the preparation.

[0046] Comparative Example In order to verify that the composite odorless smoke-suppressing asphalt of the present invention has good road performance and smoke suppression performance, the softening point and needle penetration of the modified asphalt are measured according to the "Test Procedure for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011), and the smoke production and smoke suppression rate of asphalt smoke are measured according to the "Occupational Exposure Limits for Petroleum Asphalt (Smoke) in Workshop Air (GB 18553-2001)". Taking Donghai brand 70# base asphalt as a comparative example, the modified asphalt prepared according to the above Examples 1 to 8 are respectively measured for softening point, needle penetration, smoke production and smoke suppression rate. The results are shown in Table 1 for details.

[0047] Table 1 Physical properties and smoke suppression performance of examples and comparative examples It can be seen from Table 1 that from the physical properties of the modified asphalt, the addition of all composite inhibitor combinations increased the softening point of the asphalt to varying degrees and reduced the penetration of the asphalt. The softening points of Examples 2, 3, and 7 were increased by 3°C, 2.9°C, and 1.9°C, respectively, and the penetrations of Examples 3, 7, and 4 were reduced by 32.3%, 25.3%, and 24.2%, respectively. This means that the temperature stability of the modified asphalt is improved, and the consistency is also increased. The increase in the consistency of asphalt is beneficial to improving the cohesion of the asphalt and improving the adhesion of the asphalt to the aggregate.

[0048] In addition, by comparing the smoke suppression rates of the embodiments and the comparative examples, it can be seen that the addition of IPDI significantly improves the asphalt smoke suppression effect, and the degree of improvement increases with the increase in the IPDI dosage. When the IPDI dosage is large (3%), the smoke suppression rate decreases with the increase in the nano-silicate mineral dosage. When the IPDI dosage is small (2%), the smoke suppression rate increases with the increase in the nano-silicate mineral dosage. From the perspective of the ATT-IPDI composite modified asphalt, the smoke suppression rates of Examples 2, 3, and 4 all exceed 30%, especially Example 3, with a smoke suppression rate of up to 44.67%. From the perspective of the OMMT-IPDI composite modified asphalt, the maximum smoke suppression rate is as high as 43.95%. The smoke coverage of asphalt based on PTFE filter membrane can more intuitively display the smoke suppression effect, see Figure 1 .

[0049] In summary, the odorless smoke-suppressing asphalt compounded with nano-silicate minerals and polyurethane precursors has a significant smoke-suppressing effect and improves the physical properties of asphalt. Examples 3 and 4 are excellent in smoke-suppressing effect and physical property improvement, and the smoke-suppressing rate exceeds 40%. This phenomenon may be due to the layered structure and large specific surface area of ​​nano-silicate minerals, which have a strong adsorption effect, and the addition of IPDI forms a chain network structure through a chemical reaction between the isocyanate group and the hydroxyl or other functional groups in the nano-silicate mineral / asphalt molecules, thereby further hindering the release of light components in the smoke.

Claims

1. A polyurethane precursor-nano silicate mineral composite asphalt, including base asphalt, characterized in that: It also includes a polyurethane precursor and a nano-silicate mineral, and the mass fractions of each component are as follows: Base asphalt: 100, Polyurethane precursor: 1~5, Nanosilicate minerals: 1-5.

2. The polyurethane precursor-nano silicate mineral composite asphalt according to claim 1, characterized in that: The polyurethane precursor is isophorone diisocyanate; The nano-silicate mineral is selected from at least one of nano-montmorillonite and attapulgite that have been subjected to organic modification.

3. The method for preparing the polyurethane precursor-nano silicate mineral composite asphalt according to claim 1 or 2, characterized in that: The steps include: i. In parts by mass, take 100 parts of base asphalt into a container and heat to a molten state; ii. Add 1 to 5 parts by mass of nano-silicate minerals to the molten matrix asphalt obtained in step i, and shear at a speed of 2000r / min~2500r / min for 20min~30min to form modified asphalt, to the surface of the modified asphalt and the edge of the container without obvious distribution of the modifier, and the surface of the modified asphalt remains flat; iii. Add 1 to 5 parts by mass of a polyurethane precursor to the modified asphalt obtained in step ii, stir until no bubbles are generated, and then use a high-speed shearing machine to shear at a speed of 2000r / min~2500r / min until the volume of the modified asphalt no longer expands; iv. When the volume of the modified asphalt stops expanding, the speed of the shearing machine is increased to 4000r / min~5000r / min and shearing is carried out for 45min~75min. After the shearing is completed, the modified asphalt is grown in an oven to keep it in a molten state for 2 hours to complete the preparation.