Preparation method of oil paint core-coated titanium dioxide

The titanium dioxide core encapsulation process is simplified by the oil-based coating method, solving the problems of complex titanium dioxide production and waste of resources, realizing the preparation of low-cost and low-energy consumption, and effectively utilizing titanium resources.

CN118931228APending Publication Date: 2024-11-12CHINA TITANIUM GRP JIAOZUO YUSHENG TITANIUM IND CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410991932.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing titanium dioxide production process is complex and wastes resources, resulting in tight titanium resources and rising prices. The existing coating process consumes high energy and generates waste.

Method used

The oil-based coating method is used to treat titanium dioxide and calcium carbonate through grinding and dispersion, mechanical coating, repair and modification to form a core-enclosed structure, avoiding the drying process and reducing energy consumption.

Benefits of technology

It has achieved simplification of production processes, reduced costs and eliminated waste, effectively utilized the high hiding power and whiteness characteristics of titanium dioxide to save titanium resources.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of titanium dioxide, and discloses a preparation method of oil paint core-coated titanium dioxide. Grinding and dispersing the inner core and the coating to obtain the mixed inner core and coating; mechanically coating the mixed inner core and the coating material to obtain a coating body; dispersing the coating body, repairing to obtain complete coated particles, and modifying the coated particles by using a modifier to obtain modified coated particles; s5, drying the modified coated particles to obtain core-coated titanium dioxide; the coating is titanium dioxide, and the inner core is calcium carbonate. The preparation method of the oil paint core-coated titanium dioxide is simple in production process, low in cost and free of waste generation; in the preparation process, few solvents are used, the core-coated titanium dioxide is prepared mainly in a mechanical mode, the long-time high-power-consumption drying or drying process is avoided, the cost is reduced, and energy is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium dioxide, in particular to a method for preparing oily paint-coated core titanium dioxide. Background Art

[0002] Titanium dioxide is one of the main raw materials for coatings, but it is expensive, the production process is complicated, and it is accompanied by a large amount of waste. However, its good performance has not been fully utilized in applications. According to calculations, only one-third of the particles on the surface of titanium dioxide particles play a functional role, and the core is wrapped inside and cannot play a role, which leads to a large amount of waste of titanium dioxide, a high-quality resource. With the gradual reduction of titanium resources, titanium dioxide is also in short supply and demand and its price is rising. The solution to this dilemma is to coat a layer of titanium dioxide on the surface of cheap inorganic powder to form a core-shell titanium dioxide, which can utilize the high hiding power of titanium dioxide and the high whiteness characteristics and save titanium resources.

[0003] In the prior art, the production process of titanium dioxide wrapped with core-shell is usually prepared into slurry for coating, and various surface treatment agents are used to treat the raw materials in order to make titanium dioxide better coated on the core-shell. The whole process is cumbersome, and the subsequent production in the state of slurry will inevitably consume a lot of heat energy to dry the slurry, and waste gas may be generated during the drying process.

[0004] Therefore, there is an urgent need for a method for preparing oily paint-coated core titanium dioxide to solve the above-mentioned technical problems. Summary of the invention

[0005] The purpose of the present invention is to overcome the technical problems of the prior art and develop a method for preparing oily coating-coated titanium dioxide with simple production process, low cost and no waste generation.

[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0007] A method for preparing oily paint-coated core titanium dioxide comprises the following steps:

[0008] S1, grinding and dispersing the core and the coating to obtain a mixed core and the coating;

[0009] S2, mechanically coating the mixed core and coating to obtain a coating body;

[0010] S3, dispersing the coating body and then repairing it to obtain complete coated particles;

[0011] S4, modifying the coated particles using a modifier to obtain modified coated particles;

[0012] S5, drying the modified coated particles to obtain core-coated titanium dioxide;

[0013] The coating is titanium dioxide, and the core is calcium carbonate.

[0014] Preferably, the mass percentage of the core and the coating is: 10-60% for the core and 40-90% for the coating.

[0015] Preferably, the titanium dioxide is nanometer-sized titanium dioxide; and the calcium carbonate is micrometer-sized calcium carbonate.

[0016] Preferably, the particle size of the titanium dioxide is less than 300 nm, and the particle size of the calcium carbonate is less than 2 μm.

[0017] Preferably, in step S1, an ultrafine grinder is used for grinding and dispersing, and the grinding and dispersing time is 7-15 minutes.

[0018] Specifically, the grinding and dispersion time includes but is not limited to any one of 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, and 15 min, or a range between any two of them.

[0019] Preferably, in step S2, the mechanical coating process adopts a centrifugal vibration mill with a rotation speed of 1400-1500 rpm and a coating time of 5-20 min.

[0020] Specifically, the rotation speed includes but is not limited to 1400 rpm, 1410 rpm, 1420 rpm, 1430 rpm, 1440 rpm, 1450 rpm, 1460 rpm, 1470 rpm, 1480 rpm, 1490 rpm, 1500 rpm, any one of the point values ​​or the range value between any two of them.

[0021] Specifically, the coating time includes but is not limited to any one of 5 min, 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min, and 20 min, or a range between any two of the points.

[0022] During the mechanical coating process, a mechanochemical effect occurs, which increases the surface activity of calcium carbonate under strong mechanical force and increases the number of reaction points, so that titanium dioxide particles can be evenly distributed on the surface of calcium carbonate.

[0023] Preferably, in step S3, the coating body is dispersed by high-pressure airflow; during the repair process, the dispersed coating body is placed in a container so that the coating body is in a boiling state, and the titanium dioxide is fully in contact with the uncoated calcium carbonate for adsorption and coating.

[0024] The high-pressure airflow can disperse the large flocculated particles in the coating, making it easier for the subsequent repair process.

[0025] Specifically, a fluidized bed can be used to adsorb and coat the dispersed coating body; the adsorption and coating time is 3-10 minutes, including but not limited to any point value of 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, and 10 minutes, or a range value between any two of them.

[0026] Preferably, in step S4, the modifier is a mixture of metal soap and acetic acid; the mass ratio of metal soap to acetic acid is 20:1; the amount of the modifier used is 1-5% of the mass of the coated particles, including but not limited to any one of 1%, 2%, 3%, 4%, 5% or a range between any two of them.

[0027] Specifically, the modifier is a mixture of zinc stearate and acetic acid; the mass ratio of zinc stearate to acetic acid is 20:1.

[0028] Preferably, in step S4, the modifier is evenly coated on the surface of the coated particles after being atomized.

[0029] Specifically, the coated particles are placed in a container and stirred, and the atomized modifier is evenly sprayed on the coated particles under the action of stirring, so that the modifier is evenly coated on the surface of the coated particles.

[0030] Preferably, in step S5, the drying temperature is 40-60° C., and the drying time is 5-15 min.

[0031] Specifically, the drying temperature includes but is not limited to any one of 40° C., 45° C., 50° C., 45° C., and 60° C., or a range between any two of them.

[0032] The drying time includes, but is not limited to, any one of 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, and 15 min, or a range between any two of the points.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The preparation method of the oily paint core-coated titanium dioxide powder of the present invention has a simple production process, low cost and no waste generation; less solvent is used in the preparation process, and the core-coated titanium dioxide powder is mainly prepared by mechanical means, avoiding a long-term and high-power consumption drying or drying process, reducing costs and saving energy. DETAILED DESCRIPTION

[0035] The present invention is further described below with reference to specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0036] Example 1

[0037] A method for preparing oily paint-coated core titanium dioxide comprises the following steps:

[0038] S1, grinding and dispersing the core and the coating with an ultrafine grinder for 10 min to obtain a mixed core and coating;

[0039] The mass percentage of the core and the coating is: 35% for the core and 65% for the coating; the coating is titanium dioxide and the core is calcium carbonate; the particle size of the titanium dioxide is less than 300nm and the particle size of the calcium carbonate is less than 2μm;

[0040] S2, mechanically coating the mixed core and coating to obtain a coating body; the mechanical coating process adopts a centrifugal vibration mill with a rotation speed of 1450 rpm and a coating time of 12 min;

[0041] S3, dispersing the coated body by high-pressure airflow; then using a fluidized bed to make the coated body in a boiling state, the titanium dioxide and the uncoated calcium carbonate are fully contacted for adsorption and coating, and complete coated particles are obtained; the adsorption and coating time is 7 minutes;

[0042] S4, placing the coated particles in a container and stirring them, and spraying the atomized modifier evenly on the coated particles under the action of stirring, so that the modifier is evenly coated on the surface of the coated particles, making them hydrophobic and lipophilic, and obtaining modified coated particles; the modifier is a mixture of zinc stearate and acetic acid; the mass ratio of zinc stearate to acetic acid is 20:1; the amount of the modifier used is 3% of the mass of the coated particles.

[0043] S5, drying and curing the modified coated particles at 50° C. for 10 minutes to obtain core-coated titanium dioxide.

[0044] The product obtained in this example was tested, and the obtained data met the standards of "whiteness ≥ 96.1 (powder); oil dispersibility: ≥ 6.2 (Hegman number); oil absorption: ≤ 18.3 g / 100 g".

[0045] Example 2

[0046] A method for preparing oily paint-coated core titanium dioxide comprises the following steps:

[0047] S1, grinding and dispersing the core and the coating with an ultrafine grinder for 7 minutes to obtain a mixed core and coating;

[0048] The mass percentage of the core and the coating is: 60% for the core and 40% for the coating; the coating is titanium dioxide and the core is calcium carbonate; the particle size of the titanium dioxide is less than 300nm and the particle size of the calcium carbonate is less than 2μm;

[0049] S2, mechanically coating the mixed core and coating to obtain a coating body; the mechanical coating process uses a centrifugal vibration mill with a rotation speed of 1400 rpm and a coating time of 20 min;

[0050] S3, dispersing the coated body by high-pressure airflow; then using a fluidized bed to make the coated body in a boiling state, the titanium dioxide and the uncoated calcium carbonate are fully contacted for adsorption and coating, and complete coated particles are obtained; the adsorption and coating time is 3 minutes;

[0051] S4, placing the coated particles in a container and stirring them, and spraying the atomized modifier evenly on the coated particles under the action of stirring, so that the modifier is evenly coated on the surface of the coated particles, making them hydrophobic and lipophilic to obtain modified coated particles; the modifier is a mixture of zinc stearate and acetic acid; the mass ratio of zinc stearate to acetic acid is 20:1; the amount of the modifier used is 1% of the mass of the coated particles.

[0052] S5, drying and curing the modified coated particles at 40° C. for 15 minutes to obtain core-coated titanium dioxide.

[0053] The product obtained in this example was tested, and the obtained data met the standards of "whiteness ≥ 96.1 (powder); oil dispersibility: ≥ 6.2 (Hegman number); oil absorption: ≤ 18.3 g / 100 g".

[0054] Example 3

[0055] A method for preparing oily paint-coated core titanium dioxide comprises the following steps:

[0056] S1, grinding and dispersing the core and the coating with an ultrafine grinder for 15 minutes to obtain a mixed core and coating;

[0057] The mass percentage of the core and the coating is: 10% for the core and 90% for the coating; the coating is titanium dioxide and the core is calcium carbonate; the particle size of the titanium dioxide is less than 300nm and the particle size of the calcium carbonate is less than 2μm;

[0058] S2, mechanically coating the mixed core and coating to obtain a coating body; the mechanical coating process adopts a centrifugal vibration mill with a rotation speed of 1500 rpm and a coating time of 5 min;

[0059] S3, dispersing the coated body by high-pressure airflow; then using a fluidized bed to make the coated body in a boiling state, the titanium dioxide and the uncoated calcium carbonate are fully contacted for adsorption and coating, and complete coated particles are obtained; the adsorption and coating time is 10 minutes;

[0060] S4, placing the coated particles in a container and stirring them, and spraying the atomized modifier evenly on the coated particles under the action of stirring, so that the modifier is evenly coated on the surface of the coated particles, making them hydrophobic and lipophilic, and obtaining modified coated particles; the modifier is a mixture of zinc stearate and acetic acid; the mass ratio of zinc stearate to acetic acid is 20:1; the amount of the modifier used is 5% of the mass of the coated particles.

[0061] S5, drying and curing the modified coated particles at 60° C. for 5 minutes to obtain core-coated titanium dioxide.

[0062] The product obtained in this example was tested, and the obtained data met the standards of "whiteness ≥ 96.1 (powder); oil dispersibility: ≥ 6.2 (Hegman number); oil absorption: ≤ 18.3 g / 100 g".

[0063] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A method for preparing oily paint-coated titanium dioxide, characterized in that: The following steps are involved: S1, grinding and dispersing the core and the coating to obtain a mixed core and the coating; S2, mechanically coating the mixed core and coating to obtain a coating body; S3, dispersing the coating body and then repairing it to obtain complete coated particles; S4, modifying the coated particles using a modifier to obtain modified coated particles; S5, drying the modified coated particles to obtain core-coated titanium dioxide; The coating is titanium dioxide, and the core is calcium carbonate.

2. The method for preparing an oily paint-coated core titanium dioxide according to claim 1, characterized in that: The mass percentage of the core and the coating is: 10-60% of the core and 40-90% of the coating.

3. The method for preparing an oily paint-coated core titanium dioxide according to claim 1, characterized in that: The titanium dioxide is nanometer-grade titanium dioxide; and the calcium carbonate is micrometer-grade calcium carbonate.

4. The method for preparing an oily paint-coated core titanium dioxide according to claim 3, characterized in that: The particle size of the titanium dioxide is less than 300 nm, and the particle size of the calcium carbonate is less than 2 μm.

5. The method for preparing an oily paint-coated core titanium dioxide according to claim 1, characterized in that: In the step S1, an ultrafine grinder is used for grinding and dispersing, and the grinding and dispersing time is 7-15 minutes.

6. The method for preparing an oily paint-coated core titanium dioxide according to claim 1, characterized in that: In the step S2, the mechanical coating process adopts a centrifugal vibration mill with a rotation speed of 1400-1500 rpm and a coating time of 5-20 min.

7. The method for preparing an oily paint-coated core titanium dioxide according to claim 1, characterized in that: In step S3, the coating body is dispersed by high-pressure airflow; during the repair process, the dispersed coating body is placed in a container so that the coating body is in a boiling state, and the titanium dioxide is fully in contact with the uncoated calcium carbonate for adsorption and coating.

8. The method for preparing an oily paint-coated core titanium dioxide according to claim 1, characterized in that: In the step S4, the modifier is a mixture of metal soap and acetic acid; the mass ratio of the metal soap to the acetic acid is 20:1; and the amount of the modifier used is 1-5% of the mass of the coated particles.

9. The method for preparing an oily paint-coated core titanium dioxide according to claim 8, characterized in that: In the step S4, the modifier is evenly coated on the surface of the coated particles after being atomized.

10. The method for preparing an oily paint-coated core titanium dioxide according to claim 1, characterized in that: In step S5, the drying temperature is 40-60° C., and the drying time is 5-15 minutes.

Citation Information

Cited By

  • Production method of core-coated titanium dioxide for high-solid-content coating

    CN120794002A