Organic-inorganic hybrid high-temperature-resistant solid lubricating coating and preparation method thereof

Through the combination of organic-inorganic hybrid binders and specific additives, the toughness of phosphate is enhanced and the use of Cr6+ is avoided, which solves the problem of insufficient performance of inorganic phosphate coatings in high-temperature environments, and achieves high-temperature self-lubricating and stability , suitable for gas turbine components.

CN118931231APending Publication Date: 2024-11-12DONGFANG TURBINE CO LTD

Patent Information

Application Number
CN202411091885.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing inorganic phosphate solid lubricating coatings are difficult to serve for a long time under high temperature environments, and the chromium phosphate and aluminum phosphate used in the preparation process will produce harmful Cr6+, causing pollution to the human body and the environment.

Method used

Using organic-inorganic hybrid binders and graphite powder, metal sulfide, silver powder, hexagonal boron nitride and rare earth fluoride materials, the toughness of phosphate is enhanced through the Si-O-P structure, and the dispersion of lubricating materials is improved by using organic silane. To avoid the use of Cr6+, a solid lubricating coating with high temperature resistance, stability and adhesion are prepared.

Benefits of technology

It provides a long-term service coating at room temperature to 1000°C, ensuring high-temperature friction and wear performance of gas turbine components, avoiding the harm of Cr6+, and achieving thermal stability and self-lubricity of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931231A_ABST
    Figure CN118931231A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high-temperature self-lubricating functional coatings, and discloses an organic-inorganic hybrid high-temperature-resistant solid lubricating coating and a preparation method thereof.The organic-inorganic hybrid high-temperature-resistant solid lubricating coating comprises a binder, a lubricant and a solvent, and the binder is an organic-inorganic hybrid binder; the lubricant comprises graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride and rare earth fluoride; the solvent is N, N dimethyl formamide. The organic-inorganic hybrid binder is prepared by reacting phosphoric acid, aluminum hydroxide, organosilane and a curing agent in deionized water. And the solid content is 55-60%. The prepared organic-inorganic hybrid binder has excellent self-lubricating property, wear resistance, thermal stability and good mechanical property, and has long-acting service capacity in an environment from room temperature to 1000 DEG C. The method can be applied to key moving parts such as gas turbine compressor moving blade roots and bolt fasteners, and normal service of gas turbines can be ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-temperature self-lubricating functional coatings, and in particular to an organic-inorganic hybrid high-temperature resistant solid lubricating coating and a preparation method thereof. Background Art

[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.

[0003] Mechanical wear and high temperature fatigue coupling damage is widely present in the key moving parts of gas turbines, and it has become a key common problem that seriously restricts the efficient and stable service of gas turbines. For example, the roots of gas turbine compressor moving blades, compressor guide vane bearings, bolt fasteners, etc. are in a high temperature environment for a long time and are subjected to the coupling effects of high load impact, mechanical wear and other factors for a long time. They are very prone to damage and failure, which may affect work efficiency at the least and cause major safety accidents at the worst.

[0004] The existing solution is to apply solid lubricating coatings on key moving parts to protect metals by stopping or slowing down friction and wear that may occur in high temperature environments. Compared with other surface protection technologies, solid lubricating coatings have the characteristics of low cost, simple process, and easy construction. Inorganic phosphates are widely used in the preparation of high-temperature resistant composite coatings in gas turbines, aerospace and other fields due to their good curing effect, strong bonding force and high temperature strength. However, in the preparation process of inorganic phosphate binders, both chromium phosphate and aluminum chromium phosphate will generate Cr 6+ , which is easily absorbed by the human body, can cause allergies when in contact with the skin, and even has a risk of cancer when in contact with it for a long time. In addition, chromium ions can cause serious pollution to the environment. On the other hand, existing inorganic phosphate solid lubricant coatings are difficult to effectively serve for a long time at temperatures above 600°C. Summary of the invention

[0005] The purpose of the present invention is to provide an organic-inorganic hybrid high-temperature resistant solid lubricating coating and a preparation method thereof in response to the problems of the current inorganic phosphate solid lubricating coating. The prepared coating has excellent self-lubricity, wear resistance, thermal stability and good mechanical properties. Silane and phosphate are mixed and hydrolyzed and polycondensed, and a Si-OP structure is introduced into the POP network, so that the inorganic phase and the organic phase are combined. The introduced Si-OP structure enhances the toughness of the phosphate. On the other hand, the organosilane improves the surface of the lubricating material by hydrolysis, improves the dispersibility, avoids the shortcomings of the existing technology, and can be applied to key moving parts such as the blade roots of gas turbine compressor moving blades and bolt fasteners, which can ensure the normal service of the gas turbine.

[0006] The technical solution of the present invention is as follows:

[0007] The present invention provides an organic-inorganic hybrid phosphate high-temperature solid lubricating coating, comprising a binder, a lubricant and a solvent.

[0008] The binder is an organic-inorganic hybrid binder;

[0009] The lubricant includes graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride and rare earth fluoride;

[0010] The solvent is N,N-dimethylformamide.

[0011] Organic-inorganic hybrid binders have the advantages of high temperature resistance, good stability, high toughness and adhesion, and have the ability to serve for a long time in an environment of room temperature to 1000°C.

[0012] According to a preferred embodiment, the specific formula of the lubricating coating includes the following raw materials in parts by mass: 10 to 20 parts of organic-inorganic hybrid binder, 10 to 15 parts of graphite powder, 3 to 6 parts of metal sulfide powder, 10 to 15 parts of silver powder, 3 to 5 parts of hexagonal boron nitride powder, 3 to 5 parts of rare earth fluoride powder and 50 to 65 parts of N,N-dimethylformamide (DMF).

[0013] Preferably, N,N-dimethylformamide (DMF) is preferably 50 to 61 parts.

[0014] Preferably, the graphite powder is a highly dispersible gray-black micropowder with a layered structure and a particle size of ≤5 μm.

[0015] Preferably, the metal sulfide powder is selected from at least one of molybdenum disulfide (MoS2) or tungsten disulfide (WS2), and is a black powder with a content of >98% and a particle size of ≤5 μm.

[0016] Preferably, the silver powder has a purity of 99.99% and a particle size of 0.5 to 1 μm.

[0017] Preferably, the hexagonal boron nitride (BN) is a white loose powder with a content of >98% and a particle size of ≤5 μm.

[0018] Preferably, the rare earth fluoride is selected from at least one of lanthanum trifluoride (LaF3) or cerium trifluoride (CeF3), and is a white powder with a content of >98% and a particle size of ≤5 μm.

[0019] Preferably, the organic-inorganic hybrid binder is prepared by reacting phosphoric acid, aluminum hydroxide, organic silane and a curing agent in deionized water, and has a solid content of 55-60%.

[0020] Preferably, the organic-inorganic hybrid binder is prepared from the following raw materials in parts by weight:

[0021] 30-40 parts of phosphoric acid, 8-12 parts of aluminum hydroxide, 2-4 parts of organosilane, 3-6 parts of curing agent, 40-55 parts of deionized water; wherein, phosphoric acid (H3PO4), chemical reagent, content ≥85%; Al(OH)3, white powder, content>98%; controlled molar ratio is n(P):n(Al)≥3:1.

[0022] Preferably, the organosilane is at least one of methyltrimethoxysilane, methyltriethoxysilane, hydroxysiloxane, tetraethoxysilane, methyldimethoxysilane and aminopropyltriethoxysilane, and is a chemical reagent of analytical grade.

[0023] Preferably, the curing agent is at least one of aluminum oxide (Al2O3) or zinc oxide (ZnO), and the content thereof is greater than 98%.

[0024] According to a preferred embodiment, the organic-inorganic hybrid binder is prepared according to the following method, comprising the following steps:

[0025] (1) Deionized water and phosphoric acid are added to a beaker according to the ratio, stirred and heated to 80°C, and then aluminum hydroxide is added in batches. After stirring evenly, the temperature is raised to 90-100°C, and the reaction is continued for 100-140 minutes to obtain an aluminum phosphate matrix. The obtained product is a white viscous solution.

[0026] (2) After the solution in step (1) is cooled to room temperature, the organosilane is added according to the ratio, and the mixture is stirred manually for 5 to 10 minutes, and then stirred at room temperature for 20 to 40 minutes using a magnetic stirrer. As the reaction proceeds, the organosilane and aluminum phosphate are melted together, and the stratification phenomenon disappears.

[0027] (3) Mix the curing agent with the solution of step (2) according to the ratio, stir manually for 5 to 10 minutes, and then stir with a magnetic stirrer at room temperature for 20 to 40 minutes to allow the slurry to fully react and release the gas and heat generated by the reaction. The reaction is completed to obtain an organic-inorganic hybrid binder.

[0028] The prepared organic-inorganic hybrid adhesive has strong bonding performance and high temperature resistance under high temperature conditions.

[0029] Another aspect of the present invention provides a method for preparing the organic-inorganic hybrid phosphate high-temperature solid lubricating coating, comprising the following steps:

[0030] (1) The graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride powder, rare earth fluoride powder and part of the organosilane are mixed into N,N-dimethylformamide according to the above-mentioned proportions, placed in a ball mill, and ball milled for 48 to 72 hours.

[0031] (2) The components ground and dispersed in step (1) are mixed with an organic-inorganic hybrid phosphate binder, and an appropriate amount of N,N-dimethylformamide is added to the total amount of the coating.

[0032] (3) The mixed material in step (2) is dispersed using a high-speed mechanical disperser at a speed of 4000 to 5000 r / min for 5 to 10 minutes to obtain a solid lubricating coating.

[0033] Another aspect of the present invention provides a method for preparing the organic-inorganic hybrid phosphate high-temperature solid lubricating coating, comprising the following steps:

[0034] (1) The aforementioned organic-inorganic hybrid phosphate high temperature solid lubricating coating is sprayed on the surface of the substrate after degreasing and sandblasting, with the coating being 10 to 15 cm away from the substrate surface and the spraying pressure being 0.15 to 0.25 mPa.

[0035] (2) The coating of step (1) is allowed to stand at room temperature for 2 to 8 hours to dry, then cured at 115 to 125° C. for 100 to 140 minutes, and then cured at 300 to 310° C. for 40 to 80 minutes, and then cooled to room temperature in the furnace to obtain the coating.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1. An organic-inorganic hybrid high-temperature resistant solid lubricating coating, with an organic-inorganic hybrid binder having high temperature resistance, good stability, toughness and adhesion as a binder, and graphite, metal sulfide, silver powder, hexagonal boron nitride and rare earth fluoride as lubricating phases. The selected lubricant has good matching with the organic-inorganic hybrid binder, and the substances in the lubricating phase have good synergistic effects, which solves the lubrication problem of the coating in different temperature ranges. N,N-dimethylformamide is used as a solvent, and the coating process, surface dryness and film-forming properties of the formed coating can meet the actual use requirements;

[0038] 2. An organic-inorganic hybrid high-temperature resistant solid lubricating coating, which uses an organic-inorganic hybrid binder with strong adhesion and high temperature resistance. The Si-OP structure is introduced into the POP network of the phosphate through mixed hydrolysis and polycondensation, so that the inorganic phase and the organic phase are combined. The introduced Si-OP structure enhances the toughness of the phosphate. On the other hand, the organosilane improves the surface of the lubricating material through hydrolysis and improves the dispersibility. During the curing process of the coating, the organosilane further cross-links and hydrolyzes, which can reduce the porosity of the coating and improve the density; the Al provided by the curing agent 3+ or Zn 2+ As a "bridge", it connects the phosphate ring structure and finally forms a three-dimensional network structure. The combined effect of these two aspects significantly improves the stability of the system and avoids Cr 6+The use of Cr 6+ the hazards;

[0039] 3. An organic-inorganic hybrid high-temperature resistant solid lubricating coating and a preparation method thereof. The coating preparation method and use method of the present invention are simple, the prepared coating has strong adhesion, good thermal stability, self-lubrication and wear resistance, and can provide excellent high-temperature friction and wear resistance under working conditions from room temperature to 1000°C. It is particularly suitable for key moving parts such as gas turbine compressor rotor blade roots, bolt fasteners, etc., and can ensure the long-term and stable service of the gas turbine. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the reaction process of the organic-inorganic hybrid binder of the present application. DETAILED DESCRIPTION

[0041] The specific embodiments listed in the present invention are only examples of the present invention, and the present invention is not limited to the specific embodiments described below. For those skilled in the art, any equivalent modifications and substitutions to the embodiments described below are also within the scope of the present invention. Therefore, the equal transformations and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturers are not specified for all reagents or instruments, they are all conventional products that can be purchased commercially. In order to better illustrate the present invention, numerous specific details are given in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In other embodiments, the methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the purport of the present invention.

[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art. Unless otherwise specified, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0043] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0044] Example 1

[0045] An organic-inorganic hybrid high temperature resistant solid lubricating coating, the coating is composed of the following raw materials: 10 parts of an organic-inorganic hybrid binder, 10 parts of graphite powder, 3 parts of metal sulfide powder, 10 parts of silver powder, 3 parts of hexagonal boron nitride powder, 3 parts of rare earth fluoride, and 61 parts of N,N-dimethylformamide; the above-mentioned organic-inorganic hybrid binder is prepared by reacting 30 parts of phosphoric acid, 8 parts of aluminum hydroxide, 4 parts of methyltriethoxysilane and 3 parts of aluminum oxide in 55 parts of deionized water. The specific reaction process is as follows Figure 1 .

[0046] Specific preparation method of organic-inorganic hybrid binder:

[0047] (1) Deionized water and phosphoric acid are added to a beaker according to the ratio, stirred and heated to 80°C, and then aluminum hydroxide is added in batches. After stirring evenly, the temperature is raised to 100°C, and the reaction is continued for 140 minutes to obtain an aluminum phosphate matrix. The obtained product is a white viscous solution.

[0048] (2) After the solution in step (1) is cooled to room temperature, the organosilane is added according to the ratio, and the mixture is stirred manually for 10 minutes, and then stirred at room temperature for 40 minutes using a magnetic stirrer. As the reaction proceeds, the organosilane and aluminum phosphate are melted together, and the stratification phenomenon disappears.

[0049] (3) The curing agent is mixed with the solution of step (2) according to the ratio, and after manual stirring for 10 minutes, a magnetic stirrer is used to stir for 40 minutes at room temperature to allow the slurry to fully react and release the gas and heat generated by the reaction. The reaction is completed to obtain an organic-inorganic hybrid binder.

[0050] The coating was prepared as follows:

[0051] (1) Graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride powder and rare earth fluoride powder were mixed in 50 parts of N,N-dimethylformamide and ball milled for 48 hours;

[0052] (2) After being evenly dispersed by grinding, the mixture is mixed with an organic-inorganic hybrid binder, and the remaining 11 parts of N,N-dimethylformamide are added to the total amount of the coating;

[0053] (3) Use a high-speed disperser to disperse the mixture at a speed of 4000 r / min for 5 minutes to obtain a solid lubricating coating.

[0054] How to use the paint:

[0055] (1) Use a spray gun 10 cm away from the substrate surface and spray at a spray pressure of 0.2 mPa compressed air;

[0056] (2) After spraying, the coating was allowed to stand at room temperature for 8 hours to dry, then cured at 125° C. for 100 minutes, and then cured at 310° C. for 40 minutes, and finally cooled to room temperature in the furnace to obtain the coating.

[0057] Example 2

[0058] An organic-inorganic hybrid high temperature resistant solid lubricating coating, the coating is composed of the following raw materials: 10 parts of organic-inorganic hybrid binder, 15 parts of graphite powder, 3 parts of metal sulfide powder, 15 parts of silver powder, 3 parts of hexagonal boron nitride powder, 3 parts of rare earth fluoride, 51 parts of N,N-dimethylformamide. The organic-inorganic hybrid binder is prepared by reacting 40 parts of phosphoric acid, 9 parts of aluminum hydroxide, 3 parts of hydroxysiloxane and 3 parts of aluminum oxide in 45 parts of deionized water.

[0059] Specific preparation method of organic-inorganic hybrid binder:

[0060] (1) Deionized water and phosphoric acid are added to a beaker according to the ratio, stirred and heated to 80°C, and then aluminum hydroxide is added in batches. After stirring evenly, the temperature is raised to 90°C. The reaction is continued for 100 minutes to obtain an aluminum phosphate matrix. The obtained product is a white viscous solution.

[0061] (2) After the solution in step (1) is cooled to room temperature, the organosilane is added according to the ratio, and the mixture is stirred manually for 5 minutes, and then stirred at room temperature for 20 minutes using a magnetic stirrer. As the reaction proceeds, the organosilane and aluminum phosphate are melted together, and the stratification phenomenon disappears.

[0062] (3) The curing agent is mixed with the solution of step (2) according to the ratio, and after manual stirring for 5 minutes, a magnetic stirrer is used to stir for 20 minutes at room temperature to allow the slurry to fully react and release the gas and heat generated by the reaction. The reaction is completed to obtain an organic-inorganic hybrid binder.

[0063] The coating was prepared as follows:

[0064] (1) Graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride powder and rare earth fluoride powder were mixed in 45 parts of N,N-dimethylformamide and ball milled for 72 hours;

[0065] (2) After being evenly dispersed, the mixture is mixed with an organic-inorganic hybrid binder, and the remaining 6 parts of N,N-dimethylformamide are added to the total amount of the coating;

[0066] (3) Use a high-speed disperser to disperse the mixture at a speed of 5000 r / min for 10 minutes to obtain a solid lubricating coating.

[0067] How to use the paint:

[0068] (1) Use a spray gun 15 cm away from the substrate surface and spray at a spray pressure of 0.2 mPa compressed air;

[0069] (2) After spraying, the coating was allowed to stand at room temperature for 2 hours to dry, then cured at 115° C. for 140 minutes, and then cured at 300° C. for 80 minutes, and finally cooled to room temperature in the furnace to obtain the coating.

[0070] Example 3

[0071] The invention discloses an organic-inorganic hybrid high-temperature resistant solid lubricating coating, which is composed of the following raw materials: 10 parts of an organic-inorganic hybrid binder, 10 parts of graphite powder, 6 parts of metal sulfide powder, 10 parts of silver powder, 5 parts of hexagonal boron nitride powder, 5 parts of rare earth fluoride, and 54 parts of N,N-dimethylformamide; the organic-inorganic hybrid binder is prepared by reacting 40 parts of phosphoric acid, 12 parts of aluminum hydroxide, 2 parts of tetraethoxysilane, 3 parts of aluminum oxide, and 3 parts of zinc oxide in 40 parts of deionized water.

[0072] Specific preparation method of organic-inorganic hybrid binder:

[0073] (1) Deionized water and phosphoric acid are added to a beaker according to the ratio, stirred and heated to 80°C, and then aluminum hydroxide is added in batches. After stirring evenly, the temperature is raised to 95°C, and the reaction is continued for 120 minutes to obtain an aluminum phosphate matrix. The obtained product is a white viscous solution.

[0074] (2) After the solution in step (1) is cooled to room temperature, the organosilane is added according to the ratio, and the mixture is stirred manually for 10 minutes, and then stirred at room temperature for 30 minutes using a magnetic stirrer. As the reaction proceeds, the organosilane and aluminum phosphate are melted together, and the stratification phenomenon disappears.

[0075] (3) The curing agent is mixed with the solution of step (2) according to the ratio, and after manual stirring for 5 minutes, a magnetic stirrer is used to stir for 30 minutes at room temperature to allow the slurry to fully react and release the gas and heat generated by the reaction. The reaction is completed to obtain an organic-inorganic hybrid binder.

[0076] The coating was prepared as follows:

[0077] (1) Graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride powder and rare earth fluoride powder were mixed in 45 parts of N,N-dimethylformamide and ball milled for 60 hours;

[0078] (2) After being evenly dispersed, the mixture is mixed with an organic-inorganic hybrid binder, and the remaining 9 parts of N,N-dimethylformamide are added to the total amount of the coating;

[0079] (3) Use a high-speed disperser to disperse the solid lubricating coating at a speed of 4500 r / min for 10 minutes.

[0080] How to use the paint:

[0081] (1) Use a spray gun 12 cm away from the substrate surface and spray at a spray pressure of 0.2 mPa compressed air;

[0082] (2) After spraying, the coating was allowed to stand at room temperature for 5 hours to dry, then cured at 120° C. for 120 minutes, then cured at 305° C. for 60 minutes, and finally cooled to room temperature in the furnace to obtain the coating.

[0083] Example 4

[0084] An organic-inorganic hybrid high temperature resistant solid lubricating coating, the coating is composed of the following raw materials: 20 parts of organic-inorganic hybrid binder, 10 parts of graphite powder, 3 parts of metal sulfide powder, 10 parts of silver powder, 3 parts of hexagonal boron nitride powder, 3 parts of rare earth fluoride, 51 parts of N,N-dimethylformamide. The above organic-inorganic hybrid binder is prepared by reacting 30 parts of phosphoric acid, 10 parts of aluminum hydroxide, 4 parts of methyltriethoxysilane, 4 parts of aluminum oxide and 2 parts of zinc oxide in 50 parts of deionized water, and the preparation method is the same as that of Example 3; the coating and coating preparation methods are consistent with those of Example 3.

[0085] Comparative Example 1

[0086] The coating of the comparative example is composed of the following raw materials: 10 parts of phosphate binder, 10 parts of graphite powder, 3 parts of metal sulfide powder, 10 parts of silver powder, 3 parts of hexagonal boron nitride powder, 3 parts of rare earth fluoride, and 61 parts of N,N-dimethylformamide. The phosphate binder is prepared by reacting 30 parts of phosphoric acid, 10 parts of aluminum hydroxide, 3 parts of aluminum oxide and 2 parts of zinc oxide in 55 parts of deionized water; the coating and coating preparation method are consistent with Example 1.

[0087] The test results of various properties of the coatings in the above embodiments are shown in Table 1 below:

[0088] Table 1 Coating properties

[0089]

[0090] The above-described embodiments only express the specific implementation methods of the present application, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. An organic-inorganic hybrid high temperature resistant solid lubricating coating, characterized in that: Including adhesives, lubricants and solvents, The binder is an organic-inorganic hybrid binder; The lubricant includes graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride and rare earth fluoride; The solvent is N,N-dimethylformamide.

2. The organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 1, characterized in that: The specific formula of the lubricating coating includes the following raw materials in parts by mass: 10 to 20 parts of an organic-inorganic hybrid binder, 10 to 15 parts of graphite powder, 3 to 6 parts of metal sulfide powder, 10 to 15 parts of silver powder, 3 to 5 parts of hexagonal boron nitride powder, 3 to 5 parts of rare earth fluoride powder and 50 to 65 parts of N,N-dimethylformamide.

3. An organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 1 or 2, characterized in that: The organic-inorganic hybrid binder is prepared from the following raw materials in parts by weight: 30-40 parts of phosphoric acid, 8-12 parts of aluminum hydroxide, 2-4 parts of organosilane, 3-6 parts of curing agent, and 40-55 parts of deionized water.

4. The organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 3, characterized in that: The organosilane is at least one of methyltrimethoxysilane, methyltriethoxysilane, hydroxysiloxane, tetraethoxysilane, methyldimethoxysilane and aminopropyltriethoxysilane.

5. The organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 3, characterized in that: The curing agent is at least one of aluminum oxide and zinc oxide.

6. The organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 3, characterized in that: The organic-inorganic hybrid binder is prepared according to the following method: (1) Add deionized water and phosphoric acid into a beaker according to the ratio, stir and heat to 80° C., then add aluminum hydroxide in batches, stir evenly, raise the temperature to 90-100° C., and continue the reaction for 100-140 minutes to obtain an aluminum phosphate matrix. The obtained product is a white viscous solution; (2) After the solution in step (1) is cooled to room temperature, the organosilane is added according to the ratio, and the mixture is stirred manually for 5 to 10 minutes, and then stirred at room temperature for 20 to 40 minutes using a magnetic stirrer. As the reaction proceeds, the organosilane and aluminum phosphate are melted together, and the stratification phenomenon disappears; (3) Mix the curing agent with the solution of step (2) according to the ratio, stir manually for 5 to 10 minutes, and then stir with a magnetic stirrer at room temperature for 20 to 40 minutes to allow the slurry to fully react and release the gas and heat generated by the reaction. The reaction is completed to obtain an organic-inorganic hybrid binder.

7. The organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 6, characterized in that: The solid content of the organic-inorganic hybrid binder is 55-60%.

8. The organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 3, characterized in that: Molar ratio n(P):n(Al)≥3:

1.

9. The organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 3, characterized in that: The rare earth fluoride is selected from lanthanum trifluoride and / or cerium trifluoride.

10. The method for preparing an organic-inorganic hybrid high temperature resistant solid lubricating coating according to claim 1, characterized in that: The steps include: (1) mixing the graphite powder, metal sulfide powder, silver powder, hexagonal boron nitride powder, rare earth fluoride powder and part of the organosilane in N,N-dimethylformamide according to the above-mentioned proportion, placing in a ball mill, and ball milling for 48 to 72 hours; (2) mixing the components ground and dispersed in step (1) with an organic-inorganic hybrid phosphate binder, and adding an appropriate amount of N,N-dimethylformamide to the required total amount of materials; (3) The mixed material in step (2) is dispersed using a high-speed mechanical disperser at a speed of 4000 to 5000 r / min for 5 to 10 minutes to obtain a solid lubricating coating.

Citation Information

Patent Citations

  • High temperature anti-sticking lubricating coating, and preparation method and application thereof

    CN105219257A

  • High-temperature-resistant solid lubricating coating as well as preparation and application thereof

    CN115491247A

  • Polytetrafluoroethylene / phenolic epoxy group organic bonding paint and coating and preparation method of polytetrafluoroethylene / phenolic epoxy group organic bonding paint and coating

    CN115851077A

  • PDA-BN-coated MoS2 composite material used as high-temperature-resistant lubricant additive for titanium alloy extrusion and application thereof

    CN116790307A

  • Lubricating coating based on silane modified aluminum chromium phosphate, preparation method, formed lubricating coating and preparation method of lubricating coating

    CN117143657A

Cited By

  • Lubricating coating based on silane modified aluminum chromium phosphate, preparation method, formed lubricating coating and preparation method of lubricating coating

    CN117143657A

  • Silane-modified aluminum chromate phosphate-based lubricating coating, preparation method thereof, formed lubricating coating and preparation method of lubricating coating

    CN117143657B