High-temperature-resistant building anticorrosive paint and production process thereof

By constructing a three-dimensional network structure and a modified glass fiber skeleton, the problem of failure of traditional coatings in high temperature environments is solved, and the coating is efficient and high-temperature and crack resistance is achieved, meeting the corrosion protection requirements of modern buildings.

CN118931237APending Publication Date: 2024-11-12HENAN SUNSHINE ANTICORROSIVE PAINTING CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411251305.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional paints fail in high-temperature environments, resulting in aging, peeling and corrosion of the building surface, and cannot meet the anti-corrosion and high-temperature resistance requirements of modern buildings in high-temperature, high humidity and strong corrosion environments.

Method used

The three-dimensional network structure is constructed using raw materials such as ethyl silicate, polyvinyl butyral, acrylic resin and silica sol, and modified glass fibers and nanofillers are introduced to form stable crosslinking through crosslinking reaction and physical modification treatment. Network and skeleton structure enhances the coating's high temperature resistance and crack resistance.

Benefits of technology

It significantly improves the coating's high temperature resistance, cracking and corrosion resistance, ensures that the complete structure is maintained under high temperature environments, and reduces maintenance costs and safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032390550000071
    Figure BDA0005032390550000071
  • Figure BDA0005032390550000081
    Figure BDA0005032390550000081
Patent Text Reader

Abstract

The invention relates to the technical field of building coatings, and particularly discloses a high-temperature-resistant building anticorrosive coating and a production process thereof. The high-temperature-resistant building anticorrosive paint is prepared from the following raw materials in parts by weight: 10 to 15 parts of ethyl silicate, 5 to 10 parts of polyvinyl butyral, 2 to 4 parts of polybasic acid, 10 to 20 parts of acrylic resin, 40 to 50 parts of silica sol, 10 to 15 parts of high-temperature-resistant filler, 0.2 to 0.5 part of thickening agent and 5 to 8 parts of modified glass fiber, the modified glass fiber is obtained by modifying with polydopamine; the preparation method comprises the following steps: uniformly stirring and mixing silica sol, ethyl silicate, polyvinyl butyral and acrylic resin to obtain a mixed solution; adding the polybasic acid, the high-temperature-resistant filler and the modified glass fiber into the mixed solution, uniformly stirring and mixing, and adding the thickening agent while stirring, so as to obtain the high-temperature-resistant building anticorrosive paint. The coating disclosed by the invention can be used in high-temperature and strong-corrosion industrial environments, and has the advantages of high temperature resistance and good corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of architectural coatings, and more specifically, to a high temperature resistant architectural anticorrosive coating and a production process thereof. Background Art

[0002] With the vigorous development of the modern construction industry, the use environment faced by building materials has become increasingly complex and changeable, especially in high temperature, high humidity and highly corrosive industrial environments, such as industrial plants, chimneys, thermal power plants, chemical plants and other areas, which put forward more stringent requirements on the corrosion resistance and high temperature resistance of building materials.

[0003] Although traditional coating systems show good protection and decorative effects at room temperature, they are often unable to perform well in high temperature environments. In particular, epoxy coatings, although they have excellent anti-corrosion properties and mechanical strength, are prone to changes in molecular structure under high temperature conditions, such as molecular chain breakage and re-crosslinking, which in turn cause thermal corrosion and failure of the coating, leading to aging, peeling, corrosion and other phenomena on the building surface, which seriously weakens the protective effect of the coating and increases the maintenance cost and safety hazards of the building.

[0004] Therefore, in view of the above technical difficulties, it is particularly important to develop a building coating that can simultaneously meet the requirements of high temperature resistance and corrosion resistance. Summary of the invention

[0005] In order to improve the high temperature resistance of anti-corrosion coatings, the present application provides a high temperature resistant building anti-corrosion coating and a production process thereof.

[0006] In the first aspect, the present application provides a high temperature resistant building anticorrosive coating, which adopts the following technical solution: A high temperature resistant building anticorrosive coating comprises the following raw materials in parts by weight: 10-15 parts of ethyl silicate, 5-10 parts of polyvinyl butyral, 2-4 parts of polyacid, 10-20 parts of acrylic resin, 40-50 parts of silica sol, 10-15 parts of high temperature resistant filler, 0.2-0.5 parts of thickener and 5-8 parts of modified glass fiber; the modified glass fiber is obtained by modification with polydopamine.

[0007] By adopting the above technical scheme, silica sol is a colloidal solution of nano-scale SiO2 particles uniformly dispersed in water. It combines the silicon hydroxyl groups between silica sol particles through dehydration condensation to form a silicon oxygen network structure. The coating produced has the characteristics of high temperature resistance and corrosion resistance. However, the cohesive force is too large during the dehydration condensation process, which can easily cause the coating to crack and fall off. In response to this, resin matrices such as ethyl silicate, acrylic resin and polyvinyl butyral are introduced, and a three-dimensional network structure is constructed through cross-linking and curing reactions. This structure not only reduces and disperses the cohesive force of the coating, but also promotes the close bonding between the silica sol particles and the resin matrix through the cross-linking effect of polyacids, forming a more complex and stable cross-linked network. This network structure gives the coating excellent flexibility and crack resistance, and effectively resists the cracking problem of the coating caused by temperature changes, mechanical stress and other factors.

[0008] In order to further improve the coating's anti-cracking performance, modified glass fiber is added. Its unique fiber structure is not only tightly combined with the resin matrix, but also can better disperse stress when subjected to external forces, reducing the generation and expansion of cracks. In addition, the modified glass fiber enhances the interfacial bonding force, allowing the coating to maintain a more stable structure in a high temperature environment, effectively reducing problems such as coating deformation, cracking or shedding caused by high temperature, and further improving the overall performance of the coating. The skeleton structure formed by the glass fiber in the coating not only enhances the mechanical strength and anti-cracking ability of the coating, but also promotes the uniform curing of the coating and reduces the shedding of the coating due to excessive cohesion.

[0009] Optionally, the modified glass fiber is prepared by the following steps: (1) removing impurities on the surface of the glass fiber by grinding, cleaning, and heating to obtain pretreated glass fiber; (2) The pretreated glass fiber is immersed in a dopamine solution, glutaraldehyde is added and stirred evenly, the pH of the solution is adjusted to 7.5-8.5, and the solution is immersed and reacted at 30-40°C for 8-10 hours. After filtration and separation, the solution is placed in a polyamic acid solution and stirred for 12-14 hours, and then the solid phase is collected, washed, and dried to obtain the modified glass fiber.

[0010] By adopting the above technical solution, the rough part and larger impurity particles on the surface of the glass fiber are removed by physical grinding, so that the surface is smoother, which is conducive to the uniform adhesion of the subsequent coating, and the group activity on the surface of the glass fiber is improved. The pretreated glass fiber is further immersed in a dopamine solution, and a polydopamine cross-linking layer is formed on the surface of the glass fiber by utilizing the self-polymerization reaction of dopamine to prepare a glass fiber wrapped with polydopamine. The high-temperature resistant polyamic acid is further introduced to improve the high-temperature resistance of the glass fiber, thereby improving the heat resistance of the coating. The solution pH is adjusted to the optimal Ph environment suitable for the oxidative self-polymerization reaction of dopamine. The weakly alkaline condition helps to deprotonate the phenolic hydroxyl group in the dopamine molecule and increase its reaction activity. The addition of glutaraldehyde assists the self-polymerization of dopamine to form a complex cross-linking network, further improving the toughness of the modified glass fiber.

[0011] Optionally, the concentration of the dopamine solution is 3-5 g / L.

[0012] By adopting the above technical solution, dopamine molecules are prone to oxidative self-polymerization under alkaline conditions and form a polydopamine layer on the surface of the material. A higher dopamine concentration can provide more dopamine molecules to contact the surface of the glass fiber, thereby increasing the adsorption effect. However, too high a concentration may also cause the self-polymerization reaction of dopamine molecules in the solution to be too intense, forming a large number of water-insoluble polydopamine particles, affecting their uniform distribution on the surface of the glass fiber. Therefore, the concentration of the dopamine solution is reasonably controlled so that it can be more evenly and firmly bonded to the surface of the glass fiber, thereby enhancing the modification effect.

[0013] Optionally, the mass ratio of the glass fiber, glutaraldehyde and dopamine solution added is 1:0.2:4-5; the mass ratio of the glass fiber and polyamic acid solution added is 1:2-3.

[0014] By adopting the above technical solution, the amount of each component in the glass fiber modification process is controlled within a reasonable range, thereby obtaining modified glass fiber with stable performance and reliable quality.

[0015] Optionally, the high temperature resistant filler includes nano-alumina, nano-zirconia and nano-silicon dioxide, and the weight ratio of the nano-alumina, nano-zirconia and nano-silicon dioxide added is 3-5:1-3:1.

[0016] By adopting the above technical solutions, nano-alumina and nano-zirconia, with their excellent high melting point characteristics, jointly build a high-temperature resistant skeleton in the coating system, laying a solid foundation for the application of coatings in high temperature environments. These two nanomaterials not only have extremely high melting points, but also show excellent physical and chemical stability. They can effectively prevent thermal decomposition or excessive thermal expansion of the coating under extreme temperature conditions, ensuring the structural integrity and stable performance of the coating.

[0017] Furthermore, the introduction of nano-silica significantly improves the density and hardness of the coating, thereby enhancing the high temperature resistance of the coating. The unique properties of nano-silica not only help to form a more compact and solid coating structure, but also effectively resist deformation and damage caused by high temperature, further enhancing the overall thermal stability of the coating. This multi-level combination of nanomaterials not only plays their respective advantages, but also through synergy, enables the coating to show more excellent performance in high temperature environments.

[0018] Optionally, the thickener is hydroxyethyl cellulose.

[0019] By adopting the above technical solution, hydroxyethyl cellulose can effectively increase the viscosity of the coating, help the glass fiber to be better suspended in the coating system, and reduce sedimentation and stratification. The thickening effect of hydroxyethyl cellulose is relatively mild, and it can improve the thixotropy and fluidity of the coating without introducing too much pseudoplasticity, which is beneficial to enhance the performance of the coating.

[0020] Optionally, 3-5 parts of polyvinyl acetate emulsion are also added to the raw materials.

[0021] By adopting the above technical solution, polyvinyl acetate emulsion can be used as an auxiliary film-forming substance to fill the Si-O-Si network structure of the silica sol coating, reducing film shrinkage and expansion and contraction changes caused by temperature differences, thereby improving the stability and crack resistance of the coating.

[0022] In a second aspect, the present application provides a production process for a high temperature resistant building anticorrosive coating, which adopts the following technical solution: A production process of a high temperature resistant building anticorrosive coating comprises the following steps: (1) taking silica sol, ethyl silicate, polyvinyl butyral, and acrylic resin, stirring and mixing them uniformly to obtain a mixed solution; (2) Add polyacid, high temperature resistant filler and modified glass fiber to the above mixed solution and stir to mix well, and add thickener while stirring to obtain high temperature resistant building anticorrosive coating.

[0023] In summary, this application has the following beneficial effects: 1. Since the present application adopts silica sol as the base material of the coating, and combines acrylic resin and polyvinyl butyral and other raw materials to construct a three-dimensional network structure, the nano-scale silica particles of the silica sol are tightly combined with the resin matrix through a cross-linking and curing reaction to form a stable and complex cross-linking network, which effectively resists the erosion of the coating by high temperature and corrosive environment, and significantly improves the high temperature resistance and corrosion resistance of the coating.

[0024] 2. The addition of modified glass fiber significantly enhances the coating's ability to resist cracking and deformation. The modified glass fiber is tightly combined with the resin matrix to form a skeleton structure, which effectively disperses the stress generated by the coating when it is subjected to external force or temperature changes, and reduces the generation and expansion of cracks. At the same time, the high-temperature resistant materials such as polydopamine and polyamic acid introduced during the modification process further improve the stability of the glass fiber in high-temperature environments, ensuring that the coating can still maintain its intact structure at high temperatures.

[0025] 3. The high temperature resistant fillers and auxiliary ingredients such as thickeners, hydroxyethyl cellulose and polyvinyl acetate emulsion, which are reasonably selected in the formula, jointly improve the overall stability and durability of the coating. Nanofillers not only improve the density and hardness of the coating, but also enhance the thermal stability of the coating; thickeners improve the thixotropy and fluidity of the coating, reduce sedimentation and stratification; polyvinyl acetate emulsion reduces the expansion and contraction changes caused by film shrinkage and temperature difference, thereby improving the crack resistance and stability of the coating. The synergistic effect of these ingredients enables the coating to maintain excellent performance in a variety of harsh environments. DETAILED DESCRIPTION

[0026] The present application is further described in detail below in conjunction with embodiments.

[0027] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0028] Polyamic acid solution was purchased from Hubei Langbowan Biopharmaceutical Co., Ltd., item number LBW-0114; silica sol was purchased from Yantai Hengxin Chemical Technology Co., Ltd., SiO2 30-31%, specific gravity 1.19-1.21 g / cm 3 .

[0029] Preparation examples of raw materials and / or intermediates Preparation Example 1 A modified glass fiber, the preparation of which comprises the following steps: (1) 10 kg of glass fiber was taken, ground for 30 minutes, washed with deionized water, filtered out, and heated to 120° C. to remove impurities on the surface of the glass fiber, thereby obtaining pretreated glass fiber; (2) The pretreated glass fiber was immersed in 45 kg of a dopamine solution with a concentration of 3 g / L, 2 kg of glutaraldehyde was added and stirred evenly, and then the pH of the solution was adjusted to 8.5 using a Tris-HCl solution. The solution was immersed in the solution at 30°C for 10 h, filtered and separated, and placed in a 30 kg polyamic acid solution and stirred for 12 h. The solid phase was collected, washed, and dried to obtain the modified glass fiber.

[0030] Preparation Example 2 A modified glass fiber, the preparation of which comprises the following steps: (1) 10 kg of glass fiber was taken, ground for 30 minutes, washed with deionized water, filtered out, and heated to 120° C. to remove impurities on the surface of the glass fiber, thereby obtaining pretreated glass fiber; (2) The pretreated glass fiber was immersed in 50 kg of a 5 g / L dopamine solution, 2 kg of glutaraldehyde was added and stirred evenly, and then the pH of the solution was adjusted to 7.5 using a Tris-HCl solution. The solution was immersed and reacted at 35° C. for 8 h, filtered and separated, and placed in 20 kg of a polyamic acid solution and stirred for 14 h. The solid phase was collected, washed, and dried to obtain the modified glass fiber.

[0031] Preparation Example 3 A modified glass fiber, the preparation of which comprises the following steps: (1) 10 kg of glass fiber was taken, ground for 30 minutes, washed with deionized water, filtered out, and heated to 120° C. to remove impurities on the surface of the glass fiber, thereby obtaining pretreated glass fiber; (2) The pretreated glass fiber was immersed in 40 kg of a 4 g / L dopamine solution, 2 kg of glutaraldehyde was added and stirred evenly, and then the pH of the solution was adjusted to 8 using a Tris-HCl solution. The solution was immersed and reacted at 40° C. for 9 h, filtered and separated, and placed in 25 kg of a polyamic acid solution, and the reaction was continued by stirring for 13 h. The solid phase was collected, washed, and dried to obtain the modified glass fiber.

[0032] Preparation Example 4 A modified glass fiber, which is different from Preparation Example 1 in that the concentration of the dopamine solution in this Preparation Example is 2 g / L.

[0033] Preparation Example 5 A modified glass fiber, which is different from Preparation Example 1 in that the concentration of the dopamine solution in this Preparation Example is 6 g / L.

[0034] Comparative Preparation Example 1 A modified glass fiber is different from Preparation Example 1 in that no polyamic acid solution is added during the preparation process of this Preparation Example.

[0035] Comparative Preparation Example 2 A modified glass fiber, which is different from Preparation Example 1 in that glutaraldehyde is not added during the preparation process of this Preparation Example. Example

[0036] Example 1 A high temperature resistant building anticorrosive coating, the production process is as follows: (1) 45 kg of silica sol, 10 kg of ethyl silicate, 8 kg of polyvinyl butyral, and 15 kg of acrylic resin were stirred and mixed to obtain a mixed solution; (2) Add 3 kg of citric acid (polyacid), 10 kg of high temperature resistant filler and 6.5 kg of modified glass fiber to the above mixed solution and stir to mix, and add 0.5 kg of hydroxyethyl cellulose (thickener) while stirring to obtain a high temperature resistant building anticorrosive coating. In this embodiment, the modified glass fiber prepared in Preparation Example 1 is used, and the high temperature resistant filler is nano-alumina.

[0037] Example 2 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the raw material components and their corresponding weight proportions are shown in Table 1. In this example, the modified glass fiber prepared in Preparation Example 2 is used, and the high temperature resistant filler is nano alumina.

[0038] Example 3 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the raw material components and their corresponding weight proportions are shown in Table 1. In this example, the modified glass fiber prepared in Preparation Example 3 is used, and the high temperature resistant filler is nano alumina.

[0039] Table 1 Raw materials and their weights in Examples 1-3 (kg) Example 1 Example 2 Example 3 Silica Sol 45 40 50 Ethyl silicate 10 15 12.5 Alcohol-soluble polyvinyl alcohol 8 5 10 Acrylic resin 15 10 20 Polyacid 3 2 4 High temperature resistant filler 10 15 12.5 Modified glass fiber 6.5 5 8 Thickener 0.5 0.2 0.35 Example 4 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the modified glass fiber prepared in Preparation Example 4 is used in this example.

[0040] Example 5 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the modified glass fiber prepared in Preparation Example 5 is used in this example.

[0041] Example 6 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the high temperature resistant filler added in this example is nano-alumina, nano-zirconium oxide and nano-silicon dioxide in a weight ratio of 3:1:1.

[0042] Example 7 A high temperature resistant building anticorrosive coating is different from Example 1 in that the high temperature resistant filler added in this example is nano-alumina, nano-zirconium oxide and nano-silicon dioxide in a weight ratio of 5:2:1.

[0043] Example 8 A high temperature resistant building anticorrosive coating is different from Example 1 in that the high temperature resistant filler added in this example is nano-alumina, nano-zirconium oxide and nano-silicon dioxide in a weight ratio of 4:3:1.

[0044] Example 9 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that 3 kg of polyvinyl acetate emulsion is further added in this example, and the preparation comprises the following steps: (1) 45 kg of silica sol, 10 kg of ethyl silicate, 8 kg of polyvinyl butyral, and 15 kg of acrylic resin were stirred and mixed to obtain a mixed solution; (2) Add 3 kg of citric acid (polyacid), 10 kg of high temperature resistant filler, 3 kg of polyvinyl acetate emulsion and 6.5 kg of modified glass fiber to the above mixed solution and stir to mix, and add 0.5 kg of hydroxyethyl cellulose (thickener) while stirring to obtain a high temperature resistant building anticorrosive coating. In this example, the modified glass fiber prepared in Preparation Example 1 is used, and the high temperature resistant filler is nano-alumina.

[0045] Example 10 A high temperature resistant building anticorrosive coating, which is different from Example 9 in that 5 kg of polyvinyl acetate emulsion is added in this example.

[0046] Comparative Example Comparative Example 1 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the glass fiber added in this comparative example is not modified.

[0047] Comparative Example 2 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the modified glass fiber prepared in Comparative Preparation Example 1 is added to this comparative example.

[0048] Comparative Example 3 A high temperature resistant building anticorrosive coating, which is different from Example 1 in that the modified glass fiber prepared in Comparative Preparation Example 2 is added to this comparative example.

[0049] Performance testing Detection method / test method Crack resistance: The elongation at break is tested according to the standard JC / T864-2008 Type I method.

[0050] High temperature resistance: Use a spray gun to spray the coating on a Q235 steel plate to prepare a coating sample with a thickness of 50 μm. After it is completely cured, it is placed in the air for curing for 48 hours, heated to 600°C for 6 hours, and then cooled to room temperature. The breaking elongation of the coating before and after heating is tested.

[0051] Corrosion resistance: Test acid and alkali resistance using the immersion method, referring to GB / T9274-1988 "Determination of resistance of paints and varnishes to liquid media".

[0052] Table 2 Test results Combining Examples 1-3 and Comparative Example 1 and Table 2, it can be seen that the various test data of Examples 1-3 are better than those of Comparative Example 1, indicating that the modified glass fiber prepared by the method of the present application can enhance the bonding ability with the base coating, form a network structure, tightly bond the various raw material components, effectively alleviate the stress caused by high temperature and the like, and still maintain good performance at higher temperatures.

[0053] Combining Examples 1-3 and Comparative Example 2 and Table 2, it can be seen that the test data of Examples 1-3 are better than those of Comparative Example 2, indicating that adding polyamic acid solution during the glass fiber modification process can improve its high temperature resistance, thereby improving the high temperature resistance of the coating.

[0054] Combining Examples 1-3 and Comparative Example 3 and Table 2, it can be seen that the test data of Examples 1-3 are better than those of Comparative Example 3, indicating that the addition of glutaraldehyde is beneficial to the formation of a tighter polydopamine cross-linked layer on the surface of the glass fiber, thereby improving the compatibility of the glass fiber and the base material, and at the same time improving the adhesion between the raw materials of the coating, thereby improving the high temperature resistance of the coating.

[0055] It can be seen from Examples 1-5 and Table 2 that the various test data of Examples 1-3 are better than those of Examples 4-5, indicating that the concentration of the dopamine solution in the glass fiber modification process affects the final modification effect, thereby affecting the performance of the coating. Controlling the concentration of the dopamine solution within an appropriate range can obtain a polydopamine layer uniformly distributed on the surface of the glass fiber, thereby improving the modification effect of the fiber and thus improving the high temperature resistance of the coating.

[0056] Combining Example 1 with Examples 6-8 and Table 2, it can be seen that the experimental data of Examples 6-8 are better than those of Example 1, indicating that the high-temperature resistant fillers prepared by compounding a variety of fillers can cooperate with each other to synergistically improve the high-temperature stability of the coating.

[0057] Combining Example 1 with Examples 9-10 and Table 2, it can be seen that the experimental data of Examples 9-10 are better than those of Example 1, indicating that the addition of polyvinyl acetate emulsion can reduce the expansion and contraction changes caused by temperature difference, thereby improving the high temperature resistance of the coating.

[0058] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high temperature resistant building anticorrosive coating, It is characterized in that The composition comprises the following raw materials in parts by weight: 10-15 parts of ethyl silicate, 5-10 parts of polyvinyl butyral, 2-4 parts of polyacid, 10-20 parts of acrylic resin, 40-50 parts of silica sol, 10-15 parts of high temperature resistant filler, 0.2-0.5 parts of thickener and 5-8 parts of modified glass fiber; the modified glass fiber is obtained by modification with polydopamine.

2. A high temperature resistant building anticorrosive coating according to claim 1, Features: The modified glass fiber is prepared by the following steps: (1) Removing impurities on the surface of glass fiber by grinding, cleaning and heating to obtain pretreated glass fiber; (2) Immerse the pretreated glass fiber in a dopamine solution, add glutaraldehyde and stir evenly, adjust the pH of the solution to 7.5-8.5, and soak and react at 30-40°C for 8-10 hours. Filter and separate, place in a polyamic acid solution and continue stirring and reacting for 12-14 hours, collect the solid phase, wash, and dry to obtain the modified glass fiber.

3. A high temperature resistant building anticorrosive coating according to claim 2, Features: The concentration of the dopamine solution is 3-5 g / L.

4. A high temperature resistant building anticorrosive coating according to claim 2, Features: The mass ratio of the glass fiber, glutaraldehyde and dopamine solution added is 1:0.2:4-5; the mass ratio of the glass fiber and polyamic acid solution added is 1:2-3.

5. A high temperature resistant building anticorrosive coating according to claim 1, Features: The high temperature resistant filler comprises nano-alumina, nano-zirconia and nano-silicon dioxide, and the added weight ratio of the nano-alumina, nano-zirconia and nano-silicon dioxide is 3-5:1-3:

1.

6. A high temperature resistant building anticorrosive coating according to claim 1, Features: The thickener is hydroxyethyl cellulose.

7. The high temperature resistant building anticorrosive coating according to claim 1, Features: 3-5 parts of polyvinyl acetate emulsion are also added to the raw materials.

8. A production process of a high temperature resistant building anticorrosive coating according to any one of claims 1 to 6, It is characterized in that The steps include: (1) taking silica sol, ethyl silicate, polyvinyl butyral and acrylic resin and stirring and mixing them uniformly to obtain a mixed solution; (2) Add polyacid, high temperature resistant filler and modified glass fiber to the above mixed solution and stir to mix well, while adding thickener to obtain high temperature resistant building anticorrosive coating.

Citation Information

Cited By

  • Bromine-containing epoxy resin composite material with high heat resistance and preparation method thereof