Delustering agent for indoor mixed powder coating as well as preparation method and application of delustering agent

By using step-by-step synthesis matting agents in indoor mixed powder coatings, the problems of high cost and poor versatility of matting agents are solved, and uniform matting effect and efficient powder making in different types of powder coatings are achieved, reducing epoxy The amount of resin is used to improve production efficiency and coating performance.

CN118931246APending Publication Date: 2024-11-12浙江双彩新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975503.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The matting agent in existing indoor mixed powder coatings is costly and has poor versatility, making it difficult to achieve uniform malting effect in different types of powder coatings, especially in 70/30 mixed powder coatings, and the powder making process Inadequate compatibility leads to high energy consumption and low production efficiency.

Method used

Used including 1,3,5-tris(2-hydroxyethyl) cyanuric acid, isobutyl acid, oleic acid, catalyst, epoxidation additive, hydrogen peroxide, purification solvent, high epoxy equivalent epoxy resin and mastication The matting agent of barium sulfate is prepared by step-by-step synthesis technology to form hydroxyl groups and epoxy groups with different activities to compensate for the epoxy resin and improve compatibility and curing differences with polyester resin.

Benefits of technology

A matting agent with strong versatility and excellent matting effect in 50/50, 60/40 and 70/30 mixed powder coatings has been realized, which reduces the use of E-12 epoxy resin, reduces the cost and simplifies the powder making process. , improves production efficiency, and improves the level of coating and boiling resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a delustering agent for an indoor mixed powder coating as well as a preparation method and application thereof, and belongs to the technical field of powder coatings. The technical problems that an existing delustering agent increases the cost of the powder coating and is poor in universality, poor in batch delustering stability and the like are solved. The delustering agent is prepared from the following raw materials: 1, 3, 5-tris (2-hydroxyethyl) cyanuric acid, methacrylic acid, oleic acid, methylbenzene, an epoxidation auxiliary agent, hydrogen peroxide, a purification solvent, 4, 4-dihydroxydiphenylmethane, delustering barium sulfate, a catalyst and high epoxy equivalent epoxy resin. The matting agent has hydroxyl groups and epoxy groups with different activities. The indoor mixed powder coating prepared from the delustering agent is high in delustering universality, and 10-20% of delustering effect can be stably achieved; the use amount of E-12 epoxy resin can be reduced, and the cost is reduced; a coating film is flat and smooth in appearance, high in fineness and good in water boiling resistance, and other conventional properties can meet the application requirements of the powder coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of matting agents, and in particular relates to a matting agent for indoor mixed powder coatings and a preparation method and application thereof. Background Art

[0002] Powder coatings are different from ordinary solvent-based coatings and water-based coatings. Their dispersion medium is not solvent and water, but air. They have the advantages of no solvent pollution, 100% film formation, low energy consumption, excellent environmental protection and protection, and are widely used.

[0003] At present, indoor hybrid powder coatings are mainly used for coating indoor appliances, doors and windows, cabinets and other fields. The main varieties of indoor hybrid powder coatings are 50 / 50 hybrid, 60 / 40 hybrid and 70 / 30 hybrid.

[0004] With the increasing requirements for decorative properties, the demand for indoor mixed matte powder coatings is growing. In the prior art, the matting agent used in indoor mixed matte powder coatings is mainly a carboxyl polyacrylic acid polymer, which is physically mixed with a small amount of polyepoxy acrylic acid polymer. Although the matting effect is acceptable, there are currently the following shortcomings: (1) As a matting component, the carboxyl polyacrylic acid polymer itself has a high cost, and when used in indoor powder coatings, it often consumes a large amount of E-12 epoxy resin, further increasing the cost of the powder coating; (2) When carboxyl polyacrylic acid polymers are used in indoor powder coatings, they need to be compounded with other hydroxyl polyacrylic acid or epoxy polyacrylate compounds, so their versatility is not strong, which leads to their application in different types of The matting effects of different types of powder coatings vary greatly, and the same matting agent is difficult to be used in multiple powder coatings. Therefore, different types of indoor mixed powder coatings use different types of matting agents. For example, 50 / 50 mixed powder coatings, 60 / 40 mixed powder coatings, and 70 / 30 mixed powder coatings all have obvious differences, resulting in inconvenience in application. Moreover, since the epoxy resin component in the 70 / 30 mixed powder coating only accounts for 30% of the resin mass and the content is low, while conventional carboxyl polyacrylic acid originally needs to consume epoxy resin, the matting effect of conventional matting agents used in 70 / 30 mixed powder coatings is relatively poor, and the gloss is generally above 30%. (3) The main component of the matting agent on the market is carboxyl polyacrylic acid. Due to the large difference in polarity between carboxyl polyacrylic acid and polyester resin and E-12 epoxy resin, its compatibility with other resins in powder coatings is poor, resulting in poor surface finish of the coating film due to insufficient dispersibility during the powder making process. The powder making process often requires longer mixing and grinding time, which increases energy consumption and reduces production efficiency. How to overcome the above problems and develop a matting agent that can be used in indoor hybrid powder coating systems (50 / 50 hybrid, 60 / 40 hybrid and 70 / 30 hybrid) with strong matting versatility, low overall cost and excellent surface finish is the direction of the industry's efforts. Summary of the invention

[0005] In view of this, in order to solve the above technical problems, the present invention has developed a matting agent for indoor mixed powder coatings and a preparation method and application thereof. The indoor mixed powder coating using the matting agent of the present invention not only has excellent matting effect, but can also be used for indoor 50 / 50 mixed powder coatings, 60 / 40 mixed powder coatings and 70 / 30 mixed powder coatings at the same time, has strong versatility, good surface fineness, reduces the amount of E-12 epoxy resin used, has low comprehensive cost of powder coatings, and can meet the application requirements of powder coatings in various conventional properties.

[0006] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows.

[0007] The present invention provides a matting agent for indoor mixed powder coating, which comprises the following raw materials by mole:

[0008]

[0009] It also includes a catalyst and a high epoxy equivalent type epoxy resin;

[0010] The epoxy equivalent of the high epoxy equivalent epoxy resin is 1850-1950 g / mol, and the usage is 17-20% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

[0011] Preferably, the catalyst is phosphotungstic acid, and the amount used is 1-2% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

[0012] Preferably, the high epoxy equivalent epoxy resin is a two-step high polymerization degree bisphenol A epoxy resin with a softening point of 118-125°C.

[0013] Preferably, the epoxidation aid is acetonitrile or 1,4-dioxane.

[0014] Preferably, the hydrogen peroxide is 28-32% hydrogen peroxide.

[0015] Preferably, the purification solvent is a mixed solvent of cyclohexane and ethyl acetate, and the mass ratio of the two is 2:0.8-1.

[0016] Preferably, the particle size (D97) of the matting barium sulfate is 40-45 μm.

[0017] The present invention also provides a method for preparing the matting agent for indoor mixed powder coatings, comprising the following steps:

[0018] S1. First, add the formulated amount of toluene, methacrylic acid, 1,3,5-tris(2-hydroxyethyl)cyanuric acid and catalyst into the reaction kettle, stir evenly, heat to 109-111° C., and use a water separator to perform water separation and reflux esterification reaction;

[0019] S2, sampling and testing the acid value of the reactant, when the acid value of the reactant is reduced to below 10 mgKOH / g, adding the formulated amount of oleic acid, and continuing the water separation and reflux esterification reaction at 109-111° C. using a water separator;

[0020] S3, sampling and testing the acid value of the reactant, when the acid value of the reactant is reduced to below 2 mgKOH / g, lowering the reaction temperature to 50-55°C, then adding the epoxidation aid, stirring well, and then dropping the formula amount of hydrogen peroxide, and continuing the epoxidation reaction at 50-55°C after the addition is complete;

[0021] S4, sampling and testing the iodine value of the reactants, when the iodine value of the reactants is reduced to below 2 mgKOH / g, sodium carbonate is added to adjust the pH value to 7-7.5, and then the vacuum system is started to remove toluene, epoxidation aid and water under reduced pressure at 85-92°C;

[0022] S5, when the volatile content of the material in the reaction system is less than 3%, release the vacuum system, cool to 70-75°C, add a purification solvent and stir to dissolve the material, after the material is fully dissolved, add distilled water for washing, then stand still and separate, separate the water phase to obtain an organic phase, evaporate the organic phase by vacuum thin film, obtain a reactant with a volatile content of less than 1%, and set aside;

[0023] S6, mixing, crushing and sieving the formulated amount of 4,4-dihydroxydiphenylmethane and high epoxy equivalent epoxy resin to obtain a mixed powder of 80-100 mesh for standby use;

[0024] S7, fully and uniformly mixing the reactant with a volatile content of less than 1% obtained in step S5, the mixed powder obtained in step S6 and the formulated amount of matting barium sulfate to obtain a matting agent.

[0025] Preferably, in step S3, the dripping time of the hydrogen peroxide is controlled to be 2-3 hours.

[0026] Preferably, in step S4, the vacuum degree of the vacuum system is controlled at -0.098 MPa to -0.099 MPa.

[0027] Preferably, in step S5, the amount of distilled water used is 50-60% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

[0028] Preferably, in step S5, the organic phase is subjected to vacuum thin film evaporation by a thin film evaporator, the evaporation temperature is 90-95° C., and the vacuum degree is controlled at -0.098 MPa to -0.099 MPa.

[0029] Preferably, in step S7, the reactant with a volatile content of less than 1% obtained in step S5, the mixed powder obtained in step S6 and the formulated amount of extinction barium sulfate are mixed in a high-speed mixer until uniform, and the rotation speed of the high-speed mixer is 2000-2200 rpm.

[0030] The present invention also provides application of the matting agent in indoor mixed powder coatings.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The matting agent of the present invention is mainly prepared by step-by-step synthesis using 1,3,5-tris(2-hydroxyethyl)cyanuric acid, methacrylic acid, oleic acid, toluene, epoxidation aid, hydrogen peroxide, purification solvent, catalyst, 4,4-dihydroxydiphenylmethane, high epoxy equivalent epoxy resin, matting barium sulfate, etc., and has hydroxyl and epoxy groups with different activities.

[0033] The matting agent of the present invention is used in indoor mixed powder coatings (50 / 50 mixed type, 60 / 40 mixed type and 70 / 30 mixed type), and the matting is achieved by compensating epoxy resin. The matting agent has strong versatility and excellent matting effect, and can stably achieve a matting effect of 10-20%;

[0034] At the same time, the amount of E-12 epoxy resin used can be reduced, the cost can be reduced, and the matting agent of the present invention has good compatibility with the powder coating system, the powder making process is simple, the energy consumption can be reduced and the production efficiency can be improved;

[0035] In addition, compared with the conventional carboxyl polyacrylic acid polymer matting agent that consumes epoxy resin, the matting agent product of the present invention adopts a method of compensating epoxy resin. Since the matting agent of the present invention does not contain active carboxyl groups, it not only does not consume epoxy resin during the curing process, but also provides epoxy groups and hydroxyl groups with large activity differences that can be cured with carboxyl groups in polyester resins, thereby overcoming the problem that it is difficult to achieve matting in the current 70 / 30 due to the small amount of epoxy resin used.

[0036] Since the molecular structure of the matting agent of the present invention contains epoxy groups and hydroxyl groups with different activities at the same time, the epoxy groups in the oleic acid segment have large steric hindrance and slightly low activity, while the epoxy groups on the introduced methacrylic acid segment have small steric hindrance and high activity, and the active hydroxyl groups of the hydroxyethyl groups on the cyanuric acid ring in the molecule are different from the carboxyl groups of the polyester in curing activity and epoxy groups, resulting in obvious curing differences. The functional component is further matched with an appropriate amount of 4,4-dihydroxydiphenylmethane and a high epoxy equivalent epoxy resin to further adjust the curing differences and compatibility. The active phenolic hydroxyl groups in 4,4-dihydroxydiphenylmethane and the E-12 epoxy resin are also cured to a certain extent, and the epoxy resin with a high epoxy equivalent has a large difference in epoxy equivalent and softening point from the E-12 epoxy resin, and its epoxy curing activity is also significantly different. Finally, the epoxy groups, hydroxyl groups in the matting agent molecules of the present invention and the epoxy groups in the E-12 epoxy resin have obvious differences in curing with the carboxyl polyester resin, thereby achieving effective matting. At the same time, the cyanuric acid ring in the molecular structure of the matting agent has good rigidity and high temperature resistance, and the introduction of oleic acid segments has a long-chain hydrophobic segment structure, which helps to improve the leveling grade and water boiling resistance of the coating. The coating not only has a smooth and flat surface, high fineness, and good water boiling resistance, but other conventional properties (such as impact resistance) can also meet the application requirements of powder coatings, and has better versatility and comprehensive effects. DETAILED DESCRIPTION

[0037] In order to further understand the present invention, preferred embodiments of the present invention are described below. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0038] The matting agent for indoor hybrid powder coating of the present invention comprises the following raw materials by mole: 10-14 parts of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, 11-15 parts of methacrylic acid, 10-15 parts of oleic acid, 13-18 parts of toluene, 16-21 parts of epoxidation aid, 42-55 parts of hydrogen peroxide, 40-50 parts of purification solvent, 1-1.5 parts of 4,4-dihydroxydiphenylmethane, 8-11 parts of matting barium sulfate; and also comprises a catalyst and a high epoxy equivalent type epoxy resin. The matting agent for indoor hybrid powder coating of the present invention can also be composed of the above components alone.

[0039] In the above technical scheme, the catalyst is preferably phosphotungstic acid, and the amount is preferably 1-2% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid. The epoxidation aid is preferably acetonitrile or 1,4-dioxane. Hydrogen peroxide is preferably 28-32% hydrogen peroxide. The purification solvent is preferably a mixed solvent of cyclohexane and ethyl acetate, and the mass ratio of the two is 2:0.8-1. The preferred model of extinction barium sulfate is GX-44HB, and the particle size (D97) is 40-45μm, which is purchased from Zhejiang Changxing Hongyue Non-metallic Materials Co., Ltd. The high epoxy equivalent epoxy resin is a two-step high polymerization degree bisphenol A type epoxy resin, whose epoxy equivalent is 1850-1950g / mol and softening point is 118-125°C. It is purchased from Anhui Hengtai New Materials Co., Ltd., model HT-017.

[0040] The matting agent for indoor mixed powder coating of the present invention has the appearance of white powder, epoxy equivalent: 450-490 g / mol, hydroxyl equivalent: 865-895 g / mol.

[0041] The main molecular structure of the matting agent for indoor mixed powder coatings of the present invention is as follows:

[0042]

[0043] The method for preparing the matting agent for indoor mixed powder coating of the present invention comprises the following steps:

[0044] S1. First, add the formulated amount of toluene, methacrylic acid, 1,3,5-tris(2-hydroxyethyl)cyanuric acid and catalyst into the reactor, stir evenly, heat to 109-111°C (toluene boiling point), and use a water separator to perform water separation and reflux esterification reaction;

[0045] S2, sampling and testing the acid value of the reactants, when the acid value of the reactants is reduced to below 10 mgKOH / g, it indicates that most of the methacrylic acid has been grafted, and then oleic acid is added in the formula amount, and the esterification reaction is continued at 109-111° C. (toluene boiling point) using a water separator and reflux esterification;

[0046] S3, sampling and testing the acid value of the reactants, when the acid value of the reactants is reduced to below 2mgKOH / g, it indicates that the grafting reaction of oleic acid and methacrylic acid has been completed, then the reaction temperature is reduced to 50-55°C, and then the epoxidation auxiliary agent is added, and after sufficient stirring, the formula amount of hydrogen peroxide is added dropwise, and the dropping time is controlled to be 2-3h; after the dropping is completed, the epoxidation reaction is continued at 50-55°C for heat preservation;

[0047] S4, sampling and testing the iodine value of the reactants, when the iodine value of the reactants is reduced to below 2 mgKOH / g, it means that the epoxidation has been completed, then sodium carbonate is added to neutralize the catalyst, the pH value is adjusted to 7-7.5, and then the vacuum system is started, and toluene, epoxidation aid and water are removed under reduced pressure at 85-92° C., and the vacuum degree is controlled at -0.098 MPa to -0.099 MPa;

[0048] S5, the volatile content of the material in the reaction system is less than 3%, the vacuum system is released, and then the temperature is lowered to 70-75°C, and the purification solvent is added to fully stir and dissolve the material. After the material is fully dissolved, 50-60% of the mass of 1,3,5-tris (2-hydroxyethyl) cyanuric acid distilled water is added to stir and wash at room temperature, and then static stratification is performed, and the water phase is separated to obtain an organic phase, and the organic phase is subjected to vacuum thin film evaporation by a thin film evaporator to obtain a reactant with a volatile content of less than 1%, which is set aside, and the evaporation temperature is 90-95°C, and the vacuum degree is controlled at -0.098Mpa to -0.099Mpa;

[0049] S6, mixing, crushing and sieving the formulated amount of 4,4-dihydroxydiphenylmethane and high epoxy equivalent epoxy resin to obtain a mixed powder of 80-100 mesh for standby use;

[0050] S7. Add the reactant with a volatile content of less than 1% obtained in step S5, the mixed powder obtained in step S6 and the formulated amount of matting barium sulfate into a high-speed mixer for high-speed adsorption mixing to obtain a matting agent for indoor hybrid powder coatings. The rotation speed of the high-speed mixer is 2000-2200 rpm.

[0051] The matting agent of the present invention can be used in indoor mixed powder coatings. The formula of the indoor mixed powder coating can refer to the formula of the existing common indoor mixed powder coating. It can contain polyester resin, E-12 epoxy resin, titanium dioxide, barium sulfate, leveling agent, brightener, benzoin, etc. It is suitable for 50 / 50 indoor mixed type, 60 / 40 indoor mixed type, and 70 / 30 indoor mixed type powder coatings. The addition amount of the matting agent can refer to the formula of the existing powder coating, such as the addition amount is 2.5-3.5wt%.

[0052] The terms used in the present invention generally have the meanings commonly understood by those of ordinary skill in the art, unless otherwise specified.

[0053] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below in conjunction with embodiments.

[0054] In the following examples, various processes and methods not described in detail are conventional methods known in the art. Unless otherwise specified, the materials, reagents, devices, instruments, equipment, etc. used in the following examples can be obtained from commercial sources.

[0055] Example 1

[0056] The matting agent for indoor mixed powder coatings includes the following raw materials by mole: 10 parts of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, 11 parts of methacrylic acid, 10 parts of oleic acid, 13 parts of toluene, 16 parts of acetonitrile, 42 parts of hydrogen peroxide (28% hydrogen peroxide), 40 parts of a mixed solvent of cyclohexane and ethyl acetate (the mass ratio of the two is 2:0.8), 1.5 parts of 4,4-dihydroxydiphenylmethane, and 8 parts of matting barium sulfate (GX-44HB, particle size (D97) is 43μm); it also includes phosphotungstic acid and high epoxy equivalent epoxy resin (model HT-017), the phosphotungstic acid is 1% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, and the high epoxy equivalent epoxy resin is 18% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

[0057] The method for preparing the matting agent for indoor hybrid powder coating comprises the following steps:

[0058] S1. First, add the formulated amount of toluene, methacrylic acid, 1,3,5-tris(2-hydroxyethyl)cyanuric acid and phosphotungstic acid into the reaction kettle, stir evenly, heat to 109-111°C, and use a water separator to perform water separation and reflux esterification reaction;

[0059] S2, sampling and testing the acid value of the reactant, when the acid value of the reactant is reduced to below 10 mgKOH / g, adding the formulated amount of oleic acid, and continuing the water separation and reflux esterification reaction at 109-111° C. using a water separator;

[0060] S3, sampling and testing the acid value of the reactant, when the acid value of the reactant is reduced to below 2 mgKOH / g, lowering the reaction temperature to 50-55° C., then adding acetonitrile, stirring thoroughly, and then dripping the formula amount of hydrogen peroxide, the dripping time is controlled to be 2-3 hours; after the dripping is completed, continue to keep warm at 50-55° C. for epoxidation reaction;

[0061] S4, sampling and testing the iodine value of the reactants, when the iodine value of the reactants is reduced to below 2 mgKOH / g, sodium carbonate is added to neutralize the phosphotungstic acid, the pH value is adjusted to 7-7.5, and then the vacuum system is started to remove toluene, acetonitrile and water under reduced pressure at 85-92°C, and the vacuum degree is controlled at -0.098Mpa to -0.099Mpa;

[0062] S5, the volatile content of the material in the reaction system is less than 3%, the vacuum system is released, and then the temperature is lowered to 70-75°C, a mixed solvent of cyclohexane and ethyl acetate is added to fully stir and dissolve the material, and after the material is fully dissolved, 54% of the mass of 1,3,5-tris (2-hydroxyethyl) cyanuric acid is added to distilled water at room temperature for stirring and washing, and then static stratification is performed, and the water phase is separated to obtain an organic phase, and the organic phase is subjected to vacuum thin film evaporation by a thin film evaporator to obtain a reactant with a volatile content of less than 1%, which is set aside, and the evaporation temperature is 90-95°C, and the vacuum degree is controlled at -0.098Mpa to -0.099Mpa;

[0063] S6, mixing, crushing and sieving the formulated amount of 4,4-dihydroxydiphenylmethane and high epoxy equivalent epoxy resin to obtain a mixed powder of 80-100 mesh for standby use;

[0064] S7. Add the reactant with a volatile content of less than 1% obtained in step S5, the mixed powder obtained in step S6 and the formulated amount of matting barium sulfate into a high-speed mixer for high-speed adsorption mixing to obtain a matting agent for indoor hybrid powder coatings. The rotation speed of the high-speed mixer is 2000-2200 rpm.

[0065] The matting agent for indoor hybrid powder coatings of Example 1 has the appearance of white powder, an epoxy equivalent weight of 481 g / mol, and a hydroxyl equivalent weight of 892 g / mol.

[0066] Example 2

[0067] The matting agent for indoor mixed powder coatings comprises the following raw materials by mole: 12 parts of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, 12 parts of methacrylic acid, 12 parts of oleic acid, 14 parts of toluene, 17 parts of acetonitrile, 44 parts of hydrogen peroxide (29% hydrogen peroxide), 42 parts of a mixed solvent of cyclohexane and ethyl acetate (the mass ratio of the two is 2:0.9), 1.2 parts of 4,4-dihydroxydiphenylmethane, and 9 parts of matting barium sulfate (GX-44HB, with a particle size (D97) of 43 μm); it also comprises phosphotungstic acid and high epoxy equivalent epoxy resin (model HT-017), the phosphotungstic acid is 1.5% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, and the high epoxy equivalent epoxy resin is 20% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

[0068] The preparation method of the above-mentioned matting agent for indoor hybrid powder coating is the same as that of Example 1, except for the different formulation amounts.

[0069] The matting agent for indoor hybrid powder coatings of Example 2 has the appearance of white powder, an epoxy equivalent weight of 458 g / mol, and a hydroxyl equivalent weight of 873 g / mol.

[0070] Example 3

[0071] The matting agent for indoor mixed powder coatings includes the following raw materials by mole: 13 parts of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, 13 parts of methacrylic acid, 14 parts of oleic acid, 16 parts of toluene, 19 parts of acetonitrile, 46 parts of hydrogen peroxide (28-32% hydrogen peroxide), 45 parts of a mixed solvent of cyclohexane and ethyl acetate (the mass ratio of the two is 2:0.92), 1 part of 4,4-dihydroxydiphenylmethane, and 10 parts of matting barium sulfate (GX-44HB, with a particle size (D97) of 43μm); it also includes phosphotungstic acid and high epoxy equivalent epoxy resin (model HT-017), the phosphotungstic acid is 1.8% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, and the high epoxy equivalent epoxy resin is 17% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

[0072] The preparation method of the above-mentioned matting agent for indoor hybrid powder coating is the same as that of Example 1, except for the different formulation amounts.

[0073] The matting agent for indoor hybrid powder coatings of Example 3 has the appearance of white powder, epoxy equivalent: 465 g / mol, hydroxyl equivalent: 884 g / mol.

[0074] Example 4

[0075] The matting agent for indoor mixed powder coatings includes the following raw materials by mole: 14 parts of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, 15 parts of methacrylic acid, 15 parts of oleic acid, 18 parts of toluene, 21 parts of acetonitrile, 55 parts of hydrogen peroxide (31% hydrogen peroxide), 50 parts of a mixed solvent of cyclohexane and ethyl acetate (the mass ratio of the two is 2:1), 1.1 parts of 4,4-dihydroxydiphenylmethane, and 11 parts of matting barium sulfate (GX-44HB, particle size (D97) is 43μm); it also includes phosphotungstic acid and high epoxy equivalent epoxy resin (model HT-017), phosphotungstic acid is 2% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid, and the high epoxy equivalent epoxy resin is 19% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

[0076] The preparation method of the above-mentioned matting agent for indoor hybrid powder coating is the same as that of Example 1, except for the different formulation amounts.

[0077] The matting agent for indoor hybrid powder coatings of Example 4 has the appearance of white powder, epoxy equivalent: 473 g / mol, hydroxyl equivalent: 889 g / mol.

[0078] Example 5

[0079] The matting agents of Examples 1-4 were used, and according to the indoor mixed powder coating formulation in Table 1, the materials were mixed, extruded, tableted, and crushed using a twin-screw extruder, and then the tablets were crushed and sieved (160-180 mesh) to prepare powder coatings.

[0080] Table 1 Formulation of indoor mixed powder coating of Example 5

[0081]

[0082]

[0083] Comparative Example 1

[0084] The currently commercially available carboxyl polyacrylic acid matting agent (model K7237A, purchased from Lu'an Jietongda New Materials Co., Ltd.) was used instead of the product of the present invention for plate making. According to the indoor mixed powder coating formula in Table 2, the materials were mixed, extruded, tableted, and crushed using a twin-screw extruder, and then the tablets were crushed and sieved (160-180 mesh) to make a powder coating.

[0085] Table 2 Formula of indoor mixed powder coating of comparative example 1

[0086]

[0087] In Table 1 and Table 2, the polyester resin in the 50 / 50 indoor mixed powder coating formula is a 50 / 50 mixed polyester resin, model GH-1152, purchased from Zhejiang Guanghua New Material Technology Co., Ltd.; the polyester resin in the 60 / 40 indoor mixed powder coating formula is a 60 / 40 mixed polyester resin, model GH-1162, purchased from Zhejiang Guanghua New Material Technology Co., Ltd.; the polyester resin in the 70 / 30 indoor mixed powder coating formula is a 70 / 30 mixed polyester resin, model GH-1171, purchased from Zhejiang Guanghua New Material Technology Co., Ltd.; the leveling agent model is GLP388, and the brightener model is BLC701, both from Ningbo Nanhai Chemical Co., Ltd. Other raw materials are generally commercially available.

[0088] The properties of the powder coatings prepared in Example 5 and Comparative Example 1 were tested.

[0089] The powder coating is sprayed on the surface treated tinplate substrate by using an electrostatic spray gun and cured at 180°C / 15min to obtain a powder coating.

[0090] Powder coating index testing basis: GB / T 21776-2008 "Guide to Testing Standards for Powder Coatings and Their Coatings". Leveling grade basis: PCI leveling grade, 1-10, the larger the number, the better the leveling.

[0091] The coating performance results are shown in Tables 3-5.

[0092] Table 3 Powder coating board performance (50 / 50 indoor mixed type)

[0093]

[0094] Table 4 Powder coating board performance (60 / 40 indoor mixed type)

[0095]

[0096]

[0097] Table 5 Powder coating board performance (70 / 30 indoor mixed type)

[0098]

[0099] As can be seen from Tables 3-5, the matting agent of the present invention is used for 50 / 50 indoor mixed powder coating, 60 / 40 indoor mixed powder coating and 70 / 30 indoor mixed powder coating respectively. It not only has a smooth and flat surface and good surface fineness, but also has good impact resistance and water boiling resistance, especially excellent matting effect, and stably achieves 10-20% coating matting. The matting agent product of the present invention has strong versatility. Compared with the carboxyl polyacrylic acid matting agent of Comparative Example 1, not only is the amount of the matting agent used in each powder coating formula small, but also after its use, the amount of E-12 epoxy resin is significantly reduced. The powder coating has obvious cost advantages, and the leveling grade reaches above grade 6, which is also significantly higher than the powder coatings of various types corresponding to Comparative Example 1, and the water boiling resistance is good. It has the characteristics of strong versatility, good matting performance, convenient application and excellent surface fineness.

[0100] Comparative Example 1 uses a common commercially available polyacrylic acid matting agent. Due to its insufficient versatility, when it is used in a 60 / 40 indoor mixed powder coating, the gloss reaches 34%, and when it is used in a 70 / 30 indoor mixed powder coating, the gloss reaches 41%. The matting effect is poor, and the surface fineness is slightly poor. Due to insufficient compatibility with the powder coating, its leveling grade and water boiling resistance are not as good as the product of the present invention. At the same time, since the use process requires additional consumption of E-12 epoxy resin, the amount of matting agent and E-12 epoxy resin is large, and the application effect, cost, versatility, etc. are all inferior to the product of the present invention.

[0101] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the embodiments. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. The obvious changes or modifications derived from them are still within the protection scope of the invention.

Claims

1. Matting agent, It is characterized in that In mole parts, it comprises the following ingredients: Also includes a catalyst and a high epoxy equivalent type epoxy resin; The epoxy equivalent of the high epoxy equivalent epoxy resin is 1850-1950 g / mol, and the usage is 17-20 wt % of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid.

2. The matting agent according to claim 1, It is characterized in that The catalyst is phosphotungstic acid, and the amount used is 1-2% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid; And / or, the high epoxy equivalent epoxy resin is a two-step high polymerization degree bisphenol A epoxy resin with a softening point of 118-125°C.

3. The matting agent according to claim 1, It is characterized in that The epoxidation aid is acetonitrile or 1,4-dioxane; And / or, the hydrogen peroxide is 28-32% hydrogen peroxide; And / or, the purification solvent is a mixed solvent of cyclohexane and ethyl acetate, and the mass ratio of the two is 2:0.8-1.

4. The matting agent according to claim 1, It is characterized in that The particle size of the matting barium sulfate is 40-45 μm.

5. A method for preparing a matting agent according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1. First, add the formulated amount of toluene, methacrylic acid, 1,3,5-tris(2-hydroxyethyl)cyanuric acid and catalyst into the reaction kettle, stir evenly, heat to 109-111° C., and use a water separator to perform water separation and reflux esterification reaction; S2, sampling and testing the acid value of the reactant, when the acid value of the reactant is reduced to below 10 mgKOH / g, adding the formulated amount of oleic acid, and continuing the water separation and reflux esterification reaction at 109-111° C. using a water separator; S3, sampling and testing the acid value of the reactant, when the acid value of the reactant is reduced to below 2 mgKOH / g, lowering the reaction temperature to 50-55°C, then adding the epoxidation aid, stirring well, and then dropping the formula amount of hydrogen peroxide, and continuing the epoxidation reaction at 50-55°C after the addition is complete; S4, sampling and testing the iodine value of the reactants, when the iodine value of the reactants is reduced to below 2 mgKOH / g, sodium carbonate is added to adjust the pH value to 7-7.5, and then the vacuum system is started to remove toluene, epoxidation aid and water under reduced pressure at 85-92°C; S5, when the volatile content of the material in the reaction system is less than 3%, release the vacuum system, cool to 70-75°C, add a purification solvent and stir to dissolve the material, after the material is fully dissolved, add distilled water for washing, then stand still and separate, separate the water phase to obtain an organic phase, evaporate the organic phase by vacuum thin film, obtain a reactant with a volatile content of less than 1%, and set aside; S6, mixing, crushing and sieving the formulated amount of 4,4-dihydroxydiphenylmethane and high epoxy equivalent epoxy resin to obtain a mixed powder of 80-100 mesh for standby use; S7, fully and uniformly mix the reactant with a volatile content of less than 1% obtained in step S5, the mixed powder obtained in step S6 and the formulated amount of matting barium sulfate to obtain a matting agent.

6. The method for preparing the matting agent according to claim 5, It is characterized in that In step S3, the dripping time of the hydrogen peroxide is controlled at 2-3 hours.

7. The method for preparing the matting agent according to claim 5, It is characterized in that In step S4, the vacuum degree of the vacuum system is controlled at -0.098 MPa to -0.099 MPa.

8. The method for preparing the matting agent according to claim 5, It is characterized in that In step S5, The amount of distilled water used is 50-60% of the mass of 1,3,5-tris(2-hydroxyethyl)cyanuric acid; And / or, the organic phase is subjected to vacuum thin film evaporation in a thin film evaporator, the evaporation temperature is 90-95° C., and the vacuum degree is controlled at -0.098 MPa to -0.099 MPa.

9. The method for preparing the matting agent according to claim 5, It is characterized in that In step S7, the reactant with a volatile content of less than 1% obtained in step S5, the mixed powder obtained in step S6 and the formulated amount of extinction barium sulfate are fully mixed in a high-speed mixer until they are uniform. The speed of the high-speed mixer is 2000-2200 rpm.

10. Use of the matting agent according to any one of claims 1 to 4 in indoor hybrid powder coatings.