Super-wear-resistant photo-thermal phase-change composite anti-icing coating and preparation method thereof

By combining carbon-titanium cage acrylic resin, CNTs, graphene oxide and phase change microcapsules in anti-ice coating, the problem of contradictory mechanical properties and anti-ice performance is solved, and efficient anti-ice effect and good mechanical properties are achieved. , has superhydrophobicity and photothermal properties, can effectively delay icing and achieve dynamic deicing.

CN118931278APending Publication Date: 2024-11-12SHANGHAI MARITIME UNIVERSITY

Patent Information

Application Number
CN202411027065.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There is a contradiction between the mechanical properties and the anti-ice properties of existing anti-ice coatings, and it is difficult to effectively improve the long-term effectiveness of the anti-ice performance while ensuring high mechanical strength.

Method used

The ultra-wear-resistant light-thermal phase change composite anti-icing coating is used, and the composition includes carbon-titanium cage acrylic resin, CNTs, graphene oxide, phase change microcapsules, nano-SiO2, etc. The photothermal absorption capacity is enhanced by modifying CNTs and graphene, and the photothermal absorption capacity is enhanced. Phase change microcapsules are added to the coating to improve the photothermal conversion efficiency, and combined with the high adhesion and wear resistance of the carbon-titanium cage resin, a coating with excellent adhesion resistance is formed.

Benefits of technology

It realizes the efficient anti-ice performance of the coating, with water contact angle greater than 155°, hardness higher than 2H, friction resistance of more than 800 times, and has good wear resistance, superhydrophobicity, photothermality and stain resistance, which can be passed through Sunlight irradiation rapidly increases the surface temperature and delays icing and achieves dynamic deicing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_7
    Figure SMS_7
  • Figure SMS_8
    Figure SMS_8
  • Figure SMS_9
    Figure SMS_9
Patent Text Reader

Abstract

The invention discloses a super-wear-resistant photo-thermal phase change composite anti-icing coating which comprises the following components: carbon titanium cage acrylic resin, CNTs, graphene oxide, phase change microcapsules, nano SiO2, a silane coupling agent, a fluorosilane coupling agent, a dispersing agent, a flash rust inhibitor, a flatting agent, a defoaming agent, a thickening agent, ethanol and deionized water. The raw materials are mixed, modified, stirred and the like to obtain the product. The coating product prepared by the invention effectively improves the long-term effect of the anti-icing performance of the coating while ensuring higher mechanical strength. The water contact angle is more than 155 degrees, the water rolling contact angle is less than 5 degrees, the hardness is more than 2H, and the friction resistance is 800 times. And after no illumination, the surface temperature of the coating is still maintained for 4-6 hours and is 3-5 DEG C higher than that of the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an anti-icing coating and a preparation method thereof, and in particular to an ultra-wear-resistant photothermal phase-change composite anti-icing coating and a preparation method thereof. Background Art

[0002] As a common natural phenomenon, ice and snow are widely present in life. However, in low-temperature freezing disasters, the accumulation of ice and snow causes large-scale direct damage to important basic livelihood fields such as energy and electricity, transportation, and construction facilities. Studies have shown that icing increases flight resistance by 70%, increases flight accident rate by 15%, reduces wind power efficiency by 80%, and reduces heat exchange efficiency by 20%. The anti-icing process can be divided into two stages: anti-icing and deicing. Deicing is mainly to effectively remove the ice on the surface when ice occurs on the surface of an object. Traditional methods include mechanical methods, thermal methods, chemical reagent methods, ultrasonic guided wave methods, etc., which are all active deicing methods with the intervention of external factors. There are many problems such as high energy consumption, low efficiency, high destructiveness, strong limitations, and heavy pollution. In particular, mechanical deicing, which is still widely used in aviation, wind power, transmission lines and other scenarios, will cause permanent damage to the equipment and is not an ideal application method in actual production. With the rapid development of surface coating materials and technologies, the preparation of anti-icing coatings on the surface of structures has become the main research direction of anti-icing, and has been applied in the fields of power, aviation, and ships. At present, there are two main types of anti-icing coatings. One is to prepare coatings using the unique properties of materials, such as low surface energy, heat storage and exchange, photoelectric heat, etc. The other is to construct micro-nano structures on the surface of the coating to form bionic rough structure characteristics such as super hydrophobicity and SLIPS. However, the former has problems such as insufficient anti-icing effect and poor self-repairing performance, while the latter has problems such as imbalance between mechanical properties and hydrophobic properties and serious loss of filling medium. Summary of the invention

[0003] Purpose of the invention: The purpose of the present invention is to address the contradictory defects between mechanical properties and anti-icing properties in the existing anti-icing coating technology, and to provide an ultra-wear-resistant photothermal phase change composite anti-icing coating, which effectively improves the long-term anti-icing performance of the coating while ensuring high mechanical strength.

[0004] Technical solution: On the one hand, the present invention provides a super wear-resistant photothermal phase change composite anti-icing coating, comprising the following raw materials by weight: 40-60 parts of carbon titanium cage acrylic resin, 1-5 parts of CNTs, 1-3 parts of graphene oxide, 5-10 parts of phase change microcapsules, nano-SiO 2 5-10 parts, silane coupling agent 3-5 parts, fluorosilane coupling agent 1-3 parts, dispersant 1-3 parts, anti-flash rust agent 0.5-1 parts, leveling agent 1-2 parts, defoaming agent 1-2 parts, thickener 1-3 parts, ethanol 2-5 parts, deionized water 10-20 parts.

[0005] Furthermore, the phase change microcapsules include the following raw materials in parts by weight: 6-10 parts of n-tetradecane, 2-5 parts of carbon nanotubes (CNTs), 2-4 parts of butyl acrylate (BA), 6-12 parts of methyl methacrylate (MMA), 6-10 parts of methyl laurate, 2-4 parts of sodium dodecyl sulfate (SDS), 3-5 parts of emulsifier, 2-4 parts of potassium persulfate, and 25-35 parts of deionized water.

[0006] Furthermore, the preparation method of the phase change microcapsule is as follows:

[0007] S4, adding methyl laurate, SDS and deionized water to n-tetradecane, stirring and emulsifying, and obtaining a phase change emulsion;

[0008] S5, uniformly dispersing CNTs in deionized water, stirring with ultrasonic magnetic stirring, and then sequentially adding BA, MMA, and emulsifier solution, stirring, and dispersing to obtain a shell pre-emulsion;

[0009] The phase change emulsion, BA, MMA and emulsifier solution were mixed and ultrasonically dispersed, and then the temperature was raised to 80-90°C for magnetic heating and stirring. Potassium persulfate was added dropwise, and the mixture was allowed to react at a constant temperature. Then potassium persulfate and shell pre-emulsion were added, and the mixture was allowed to react at a constant temperature. Finally, the mixture was centrifuged at high speed at room temperature, and the mixture was washed and filtered with deionized water to obtain the n-tetradecane / CNTs phase change energy storage microcapsules.

[0010] Furthermore, the carbon titanium cage acrylic resin is D008H carbon titanium cage water-based acrylic resin; the CNTs have an outer diameter of 10-20 nm and a length of 5-15 μm; the nano-SiO 2 Amino spherical SiO 2 Nanoparticles.

[0011] Furthermore, the diameter-to-thickness ratio of the graphene oxide is greater than 2000 μm. 2 / g; the fluorosilane coupling agent is one of DY-F0301 and DY-F1702; the silane coupling agent is one of KH-550 and KH-570; the fluorosilane coupling agent is one of DY-F0301 and DY-F1702.

[0012] Furthermore, the emulsifier is one of DC-106 and OP-10; and the dispersant is an aqueous dispersant.

[0013] Furthermore, the aqueous dispersant is one of F497, F4190, Synde-147B, and Synde-147T.

[0014] Furthermore, the anti-flash rust agent is one of Rolox-X151 and PC-37; the defoaming agent is one of Synde-136, Synde-138 and Synde-137E; the leveling agent is one of Synde-1248, Synde-122X, 6008, One of a kind HX 425.

[0015] Furthermore, the thickener is one of sodium carboxymethyl cellulose, carbomer emulsion SF-R, and EM-108.

[0016] Another aspect of the present invention provides a method for preparing the ultra-wear-resistant photothermal phase-change composite anti-icing coating, comprising the following steps:

[0017] (1): CNTs and graphene oxide are respectively added into ethanol and fluorosilane coupling agent for dispersion, then ultrasonically treated, and finally dried to obtain fluorosilicone-modified CNTs and fluorosilicone-modified graphene oxide;

[0018] (2): Modified CNTs, modified graphene oxide, nano-SiO 2 , phase change microcapsules are sequentially added into deionized water for dispersion, and then carbon titanium cage acrylic resin is added, and high-speed dispersion is performed at 1000-1200 r / min for 20-30 mins to obtain a mixed solution;

[0019] (3): Add silane coupling agent, dispersant, anti-rust agent, defoaming agent and leveling agent to the mixed liquid in sequence, disperse uniformly at high speed at 800-1000r / min for 30-40mins, and finally add thickener to adjust the viscosity to prepare an ultra-wear-resistant photothermal phase change composite anti-icing coating.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The matrix resin of the present invention is a hyperbranched carbon titanium cage acrylic resin, which has strong adhesion, wear resistance, corrosion resistance, aging resistance, and amphiphilicity, and the surface itself has a micro-protrusion structure, and at the same time enhances the micro-nano-level papillary rough structure to give the coating surface excellent anti-adhesion ability, promote the rolling and shedding of water molecules and ice layers, and the coating composite filler enhances the hydrophobicity of the coating, and its water contact angle is greater than 155°, the water rolling contact angle is less than 5°, the hardness is greater than 2H, the friction resistance is more than 800 times, and it has good wear resistance, super hydrophobicity, photothermal property, and antifouling property. The static water contact angle reaches 158°, and the dynamic water contact angle is as low as 3°.

[0022] 2. In terms of photothermal deicing, the graphene-composite carbon nanotubes in the coating increase the light absorption specific surface area and improve the photothermal conversion energy absorption characteristics of the coating. The phase change microcapsules effectively improve the photothermal absorption and conversion efficiency after being wrapped and modified by carbon nanotubes, and the heat release performance of the phase change material is enhanced. Through the irradiation of sunlight, the surface temperature of the coating can be quickly increased to delay ice formation, melt the ice, form spontaneous jumps, and realize dynamic deicing. The ice delay is more than 1200s, and the surface temperature of the coating remains 3-5℃ higher than the environment for 4-6 hours without light.

[0023] 3. The carbon-titanium cage resin composite graphene and nano-SiO2 with strong mechanical properties further improve the mechanical properties of the coating, and still maintain 151° and 5° after 50 frictions. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be further described below.

[0025] Example 1

[0026] The method for preparing the ultra-wear-resistant photothermal phase-change composite anti-icing coating of this embodiment comprises the following steps:

[0027] Step 1: Add 2 parts of CNTs and 1 part of graphene oxide to 2 parts of ethanol and 1 part of fluorosilane coupling agent respectively, disperse at 1000r / min for 30mins, then ultrasonically treat for 20mins, and finally dry to obtain fluorosilicone-modified CNTs and fluorosilicone-modified graphene;

[0028] Step 2: Fluorine-silicon modified CNTs, fluorine-silicon modified graphene, 5 parts of nano-SiO 2 The particles and 5 parts of phase change microcapsules were sequentially added to 10 parts of deionized water and dispersed at 800 r / min for 30 minutes, and then 40 parts of carbon titanium cage acrylic resin were added and dispersed at 1000 r / min for 30 minutes to obtain a mixed solution;

[0029] Step 3: Add 3 parts of silane coupling agent, 1 part of dispersant, 0.5 parts of anti-rust agent, 1 part of defoaming agent, and 1 part of leveling agent to the mixed liquid in sequence, stir and disperse at 800r / min for 1 hour, and finally add 2 parts of thickener to adjust the viscosity to prepare the anti-icing coating.

[0030] The preparation method of phase change microcapsules includes:

[0031] S1. Add 6 parts of methyl laurate, 2 parts of SDS and 25 parts of deionized water to 6 parts of n-tetradecane, stir and emulsify at 400 r / min for 3 hours to obtain a phase change emulsion.

[0032] S2. Disperse 2 parts of CNTs uniformly in deionized water, and stir at 1200 r / min ultrasonic magnetic stirring for 30 mins. Then add 1 part of BA, 3 parts of MMA, and 1 part of emulsifier in sequence, stir at 1500 r / min high speed for 20 mins, and then disperse by ultrasonic for 20 mins to obtain a shell pre-emulsion.

[0033] S3, after mixing the phase change emulsion, 1 part of BA, 3 parts of MMA, and 1 part of emulsifier solution and ultrasonically dispersing for 30 minutes, the mixture was heated to 80°C at 1200r / min by magnetic heating and stirring, and 1 part of potassium persulfate initiator was added dropwise, and the mixture was allowed to stand at a constant temperature for 1 hour. Then 1 part of potassium persulfate solution and shell pre-emulsion were added. The mixture was allowed to stand at a constant temperature for 3 hours, and finally centrifuged at 1500r / min at room temperature, and the n-tetradecane / CNTs phase change energy storage microcapsules were obtained by washing and filtering with deionized water and anhydrous ethanol.

[0034] Wherein, the carbon-titanium cage acrylic resin is D008H carbon-titanium cage water-based acrylic resin;

[0035] Wherein, the outer diameter of the carbon nanotube is 10-20nm, and the length is 5-15μm;

[0036] Wherein, the nano-SiO 2 Amino spherical SiO with a particle size of 50-300nm 2 Nanoparticles;

[0037] Wherein, the graphene has a diameter-to-thickness ratio of >2000m 2 / g of graphene oxide;

[0038] Wherein, the silane coupling agent is KH-550;

[0039] Wherein, the fluorosilane coupling agent is DY-F0301;

[0040] Wherein, the emulsifier is DC-106;

[0041] Wherein, the dispersant is an aqueous dispersant Synde-147B;

[0042] Wherein, the anti-flash rust agent is Rolox-X151;

[0043] Wherein, the defoaming agent is Synde-138;

[0044] Wherein, the thickener is sodium carboxymethyl cellulose;

[0045] Wherein, the leveling agent is 6008.

[0046] Example 2

[0047] The method for preparing the ultra-wear-resistant photothermal phase-change composite anti-icing coating of this embodiment comprises the following steps:

[0048] Step 1: Add 3 parts of CNTs and 2 parts of graphene oxide to 3 parts of ethanol and 2 parts of fluorosilane coupling agent respectively, disperse at 1000r / min for 30mins, then ultrasonically treat for 20mins, and finally dry to obtain fluorosilicone-modified CNTs and fluorosilicone-modified graphene;

[0049] Step 2: Fluorine-silicon modified CNTs, fluorine-silicon modified graphene, 8 parts of nano-SiO 2 The particles and 8 parts of phase change microcapsules were sequentially added to 15 parts of deionized water and dispersed at 800 r / min for 30 minutes, and then 50 parts of carbon titanium cage acrylic resin were added and dispersed at 1000 r / min for 30 minutes to obtain a mixed solution;

[0050] Step 3: Add 3 parts of silane coupling agent, 2 parts of dispersant, 1 part of anti-rust agent, 1 part of defoaming agent, and 1 part of leveling agent to the mixed liquid in sequence, stir and disperse at 800r / min for 1h, and finally add 1 part of thickener to adjust the viscosity to prepare the anti-icing coating.

[0051] The preparation method of phase change microcapsules includes:

[0052] S1. Add 8 parts of methyl laurate, 3 parts of SDS and 30 parts of deionized water to 8 parts of n-tetradecane, stir and emulsify at 400 r / min for 3 hours to obtain a phase change emulsion.

[0053] S2. Add 4 parts of CNT to deionized water, and disperse them with ultrasonic magnetic stirring at 1200r / min for 30mins. Then add 3 parts of BA, 6 parts of MMA, and 2 parts of emulsifier in sequence, stir at 1500r / min for 20mins, and then ultrasonically disperse for 20mins to obtain a shell pre-emulsion. S3. Mix the phase change emulsion, 1 part of BA, 3 parts of MMA, and 1 part of emulsifier solution and ultrasonically disperse them for 30min, then stir at 1200r / min magnetic heating and stirring to 80°C, add 1 part of potassium persulfate initiator dropwise, and let it stand at a constant temperature for 1h. Then add 2 parts of potassium persulfate solution and shell pre-emulsion. Let it stand at a constant temperature for 3h, and finally centrifuge at 1500r / min at room temperature, wash and filter with deionized water and anhydrous ethanol to obtain n-tetradecane / CNTs phase change energy storage microcapsules.

[0054] Wherein, the carbon-titanium cage acrylic resin is D008H carbon-titanium cage water-based acrylic resin;

[0055] Wherein, the outer diameter of the carbon nanotube is 10-20nm, and the length is 5-15μm;

[0056] Wherein, the nano-SiO 2Amino spherical SiO with a particle size of 50-300nm 2 Nanoparticles;

[0057] Wherein, the graphene has a diameter-to-thickness ratio of >2000m 2 / g of graphene oxide;

[0058] Wherein, the silane coupling agent is KH-550;

[0059] Wherein, the fluorosilane coupling agent is DY-F0301;

[0060] Wherein, the emulsifier is DC-106;

[0061] Wherein, the dispersant is an aqueous dispersant Synde-147B;

[0062] Wherein, the anti-flash rust agent is Rolox-X151;

[0063] Wherein, the defoaming agent is Synde-138;

[0064] Wherein, the thickener is sodium carboxymethyl cellulose;

[0065] Wherein, the leveling agent is 6008.

[0066] Example 3

[0067] The method for preparing the ultra-wear-resistant photothermal phase-change composite anti-icing coating of this embodiment comprises the following steps:

[0068] Step 1: Add 1 part of CNTs and 3 parts of graphene oxide to 5 parts of ethanol and 3 parts of fluorosilane coupling agent respectively, disperse at 1000r / min for 30mins, then ultrasonically treat for 20mins, and finally dry to obtain fluorosilicone-modified CNTs and fluorosilicone-modified graphene;

[0069] Step 2: Fluorine-silicon modified CNTs, fluorine-silicon modified graphene, 10 parts of nano-SiO 2 The particles and 10 parts of phase change microcapsules were sequentially added to 20 parts of deionized water and dispersed at 800 r / min for 30 minutes, and then 50 parts of carbon titanium cage acrylic resin were added and dispersed at 1000 r / min for 30 minutes to obtain a mixed solution;

[0070] Step 3: Add 4 parts of silane coupling agent, 3 parts of dispersant, 1 part of anti-rust agent, 2 parts of defoaming agent, and 2 parts of leveling agent to the mixed liquid in sequence, stir and disperse at 800r / min for 1h, and finally add 1 part of thickener to adjust the viscosity to prepare the anti-icing coating.

[0071] The preparation method of phase change microcapsules includes:

[0072] S1. Add 10 parts of methyl laurate, 3 parts of SDS and 35 parts of deionized water to 8 parts of n-tetradecane, stir and emulsify at 400r / min for 3h to obtain a phase change emulsion. S2. Add 2 parts of CNT to deionized water, and disperse at 1200r / min ultrasonic magnetic stirring for 30mins. Then add 2 parts of BA, 6 parts of MMA, and 2 parts of emulsifier in turn, stir at 1500r / min for 20mins, and then ultrasonically disperse for 20mins to obtain a shell pre-emulsion. S3. Mix the phase change emulsion, 1 part of BA, 3 parts of MMA, and 1 part of emulsifier solution and ultrasonically disperse for 30min, then magnetically heat and stir at 1200r / min to 80°C, add 1 part of potassium persulfate initiator, and let it stand at constant temperature for 1h. Then add 2 parts of potassium persulfate solution and shell pre-emulsion. The reaction was allowed to stand at a constant temperature for 3 h, and finally the mixture was centrifuged at 1500 r / min at room temperature. The mixture was washed with deionized water and anhydrous ethanol and filtered to obtain n-tetradecane / CNTs phase change energy storage microcapsules.

[0073] Wherein, the carbon-titanium cage acrylic resin is D008H carbon-titanium cage water-based acrylic resin;

[0074] Wherein, the outer diameter of the carbon nanotube is 10-20nm, and the length is 5-15μm;

[0075] Wherein, the nano-SiO 2 Amino spherical SiO with a particle size of 50-300nm 2 Nanoparticles;

[0076] Wherein, the graphene has a diameter-to-thickness ratio of >2000m 2 / g of graphene oxide.

[0077] Wherein, the silane coupling agent is KH-550;

[0078] Wherein, the fluorosilane coupling agent is DY-F0301;

[0079] Wherein, the emulsifier is DC-106;

[0080] Wherein, the dispersant is an aqueous dispersant Synde-147B;

[0081] Wherein, the anti-flash rust agent is Rolox-X151;

[0082] Wherein, the defoaming agent is Synde-138;

[0083] Wherein, the thickener is sodium carboxymethyl cellulose;

[0084] Wherein, the leveling agent is 6008.

[0085] Example 4

[0086] The method for preparing the ultra-wear-resistant photothermal phase-change composite anti-icing coating of this embodiment comprises the following steps:

[0087] Step 1: Add 1 part of CNTs and 3 parts of graphene oxide to 5 parts of ethanol and 3 parts of fluorosilane coupling agent respectively, disperse at 1000r / min for 30mins, then ultrasonically treat for 20mins, and finally dry to obtain fluorosilicone-modified CNTs and fluorosilicone-modified graphene;

[0088] Step 2: Fluorine-silicon modified CNTs, fluorine-silicon modified graphene, 10 parts of nano-SiO 2 The particles and 10 parts of phase change microcapsules were sequentially added to 20 parts of deionized water and dispersed at 800 r / min for 30 minutes, and then 50 parts of carbon titanium cage acrylic resin were added and dispersed at 1000 r / min for 30 minutes to obtain a mixed solution;

[0089] Step 3: Add 4 parts of silane coupling agent, 3 parts of dispersant, 1 part of anti-rust agent, 2 parts of defoaming agent, and 2 parts of leveling agent to the mixed liquid in sequence, stir and disperse at 800r / min for 1h, and finally add 1 part of thickener to adjust the viscosity to prepare the anti-icing coating.

[0090] The preparation method of phase change microcapsules includes:

[0091] S1. Add 10 parts of methyl laurate, 3 parts of SDS and 30 parts of deionized water to 8 parts of n-tetradecane, stir and emulsify at 400 r / min for 3 hours to obtain a phase change emulsion.

[0092] S2. Add 2 parts of CNTs to deionized water, disperse them with ultrasonic magnetic stirring at 1200 r / min for 30 mins. Then add 2 parts of BA, 6 parts of MMA, and 3 parts of emulsifier in sequence, stir at 1500 r / min for 20 mins, and then disperse them with ultrasonic stirring for 20 mins to obtain a shell pre-emulsion.

[0093] S3, after mixing the phase change emulsion, 1 part of BA, 3 parts of MMA, and 2 parts of emulsifier solution and ultrasonically dispersing for 30 minutes, the mixture was stirred at 1200r / min and heated to 80°C, and 2 parts of potassium persulfate initiator were added dropwise, and the mixture was allowed to stand at a constant temperature for 1 hour. Then 2 parts of potassium persulfate solution and shell pre-emulsion were added. The mixture was allowed to stand at a constant temperature for 3 hours, and finally centrifuged at 1500r / min at room temperature, and the n-tetradecane / CNTs phase change energy storage microcapsules were obtained by washing with deionized water and anhydrous ethanol and filtering.

[0094] Wherein, the carbon-titanium cage acrylic resin is D008H carbon-titanium cage water-based acrylic resin;

[0095] Wherein, the outer diameter of the carbon nanotube is 10-20nm, and the length is 5-15μm;

[0096] Wherein, the nano-SiO 2 Amino spherical SiO with a particle size of 50-300nm 2 Nanoparticles;

[0097] Wherein, the graphene has a diameter-to-thickness ratio of >2000m 2 / g of graphene oxide.

[0098] Wherein, the silane coupling agent is KH-550;

[0099] Wherein, the fluorosilane coupling agent is DY-F0301;

[0100] Wherein, the emulsifier is DC-106;

[0101] Wherein, the dispersant is an aqueous dispersant Synde-147B;

[0102] Wherein, the anti-flash rust agent is Rolox-X151;

[0103] Wherein, the defoaming agent is Synde-138;

[0104] Wherein, the thickener is sodium carboxymethyl cellulose;

[0105] Wherein, the leveling agent is 6008.

[0106] The difference between Comparative Example 1 and Example 3 is that no microcapsules, CNTs, graphene photothermal phase change material, or fluorosilane coupling agent is added.

[0107] The difference between Comparative Example 2 and Example 2 is that the resin is conventional unmodified acrylic resin, and no mechanical performance strengthening material nano-SiO 2 .

[0108] Table 1

[0109]

[0110]

[0111] Table 2

[0112]

[0113] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.

Claims

1. A super wear-resistant photothermal phase change composite anti-icing coating, characterized by: The invention comprises the following raw materials in parts by weight: 40-60 parts of carbon-titanium cage acrylic resin, 1-5 parts of CNTs, 1-3 parts of graphene oxide, 5-10 parts of phase change microcapsules, 5-10 parts of nano-SiO2, 3-5 parts of silane coupling agent, 1-3 parts of fluorosilane coupling agent, 1-3 parts of dispersant, 0.5-1 parts of anti-flash rust agent, 1-2 parts of leveling agent, 1-2 parts of defoaming agent, 1-3 parts of thickener, 2-5 parts of ethanol and 10-20 parts of deionized water.

2. The ultra-wear-resistant photothermal phase-change composite anti-icing coating according to claim 1 is characterized in that: The phase-change microcapsules include the following raw materials in parts by weight: 6-10 parts of n-tetradecane, 2-5 parts of carbon nanotubes (CNTs), 2-4 parts of butyl acrylate (BA), 6-12 parts of methyl methacrylate (MMA), 6-10 parts of methyl laurate, 2-4 parts of sodium dodecyl sulfate (SDS), 3-5 parts of emulsifier, 2-4 parts of potassium persulfate, and 25-35 parts of deionized water.

3. The ultra-wear-resistant photothermal phase-change composite anti-icing coating according to claim 2 is characterized in that: The preparation method of the phase change microcapsule is as follows: S1. Add methyl laurate, SDS and deionized water to n-tetradecane, stir and emulsify to obtain a phase change emulsion; S2, uniformly dispersing CNTs in deionized water, stirring with ultrasonic magnetic stirring, and then sequentially adding BA, MMA, and emulsifier solution, stirring, and dispersing to obtain a shell pre-emulsion; S3. After the phase change emulsion, BA, MMA and emulsifier solution are mixed and ultrasonically dispersed, the temperature is raised to 80-90°C and magnetically heated and stirred, potassium persulfate is added dropwise, and the reaction is allowed to stand at a constant temperature. Then potassium persulfate and shell pre-emulsion are added, and the reaction is allowed to stand at a constant temperature. Finally, high-speed centrifugation is performed at room temperature, and the n-tetradecane / CNTs phase change energy storage microcapsules are obtained after washing and filtration with deionized water.

4. The ultra-wear-resistant photothermal phase-change composite anti-icing coating according to claim 1, characterized in that: The carbon titanium cage acrylic resin is D008H carbon titanium cage water-based acrylic resin; the CNTs have a tube outer diameter of 10-20 nm and a tube length of 5-15 μm; and the nano-SiO2 is amino spherical SiO2 nanoparticles.

5. The ultra-wear-resistant photothermal phase-change composite anti-icing coating according to claim 1 is characterized in that: The diameter-to-thickness ratio of the graphene oxide is greater than 2000 μm. 2 / g; the fluorosilane coupling agent is one of DY-F0301 and DY-F1702; the silane coupling agent is one of KH-550 and KH-570; the fluorosilane coupling agent is one of DY-F0301 and DY-F1702.

6. The ultra-wear-resistant photothermal phase-change composite anti-icing coating according to claim 1, characterized in that: The emulsifier is one of DC-106 and OP-10; the dispersant is an aqueous dispersant.

7. The ultra-wear-resistant light-thermal phase-change composite anti-icing coating according to claim 6 is characterized in that: The aqueous dispersant is one of F497, F4190, Synde-147B and Synde-147T.

8. The ultra-wear-resistant photothermal phase-change composite anti-icing coating according to claim 1, characterized in that: The anti-flash rust agent is one of Rolox-X151 and PC-37; the defoaming agent is one of Synde-136, Synde-138 and Synde-137E; the leveling agent is Synde-1248, Synde-122X, HX 6008, One of the HX425.

9. The ultra-wear-resistant photothermal phase-change composite anti-icing coating according to claim 1, characterized in that: The thickener is one of sodium carboxymethyl cellulose, carbomer emulsion SF-R and EM-108.

10. The method for preparing the super wear-resistant photothermal phase change composite anti-icing coating according to claim 1, characterized in that: The following steps are involved: (1): CNTs and graphene oxide are respectively added into ethanol and fluorosilane coupling agent for dispersion, then ultrasonically treated, and finally dried to obtain fluorosilicone-modified CNTs and fluorosilicone-modified graphene oxide; (2): Modified CNTs, modified graphene oxide, nano-SiO2, and phase change microcapsules are sequentially added to deionized water for dispersion, and then carbon titanium cage acrylic resin is added, and high-speed dispersion is performed at 1000-1200 r / min for 20-30 mins to obtain a mixed solution; (3): Add silane coupling agent, dispersant, anti-rust agent, defoaming agent and leveling agent to the mixed liquid in sequence, disperse uniformly at high speed at 800-1000r / min for 30-40mins, and finally add thickener to adjust the viscosity to prepare an ultra-wear-resistant photothermal phase change composite anti-icing coating.

Citation Information

Patent Citations

  • High-latent-heat-value phase change microcapsule with photo-thermal conversion effect and preparation method of high-latent-heat-value phase change microcapsule

    CN113663615A

  • Preparation method of fluoride-free wear-resistant super-hydrophobic anti-icing coatinglayer with photothermal effect

    CN114058227A

  • Bionic frost preventing and removing material as well as preparation method and application thereof

    CN115011225A

  • Water-based heavy anti-corrosion coating and preparation method thereof

    CN118064058A

Cited By

  • Wear-resistant rubber-plastic composite material for high-pressure air pipe and production method thereof