Polymer-based cement waterproof coating and preparation process thereof

By using cement waterproof coatings composed of fluoropolyacrylate emulsion and modified silica powder, the problem of degradation of waterproof performance of existing cement waterproof coatings is solved, and high-performance waterproofing, durability and mechanical performance improvements are achieved.

CN118931299AInactive Publication Date: 2024-11-12SHENZHEN HUAZHI PURIFICATION TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411166913.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cement waterproof coatings may degrade their waterproof performance under long-term soaking or extreme climate conditions, making it difficult to meet the high standards of waterproof materials in modern buildings.

Method used

A polymer-based cement waterproof coating composed of fluorinated polyacrylate emulsion, modified silica powder, filler components, coupling agent, defoaming agent, water reducing agent and composite curing agent is prepared by emulsion polymerization method Fluorinated polyacrylate emulsion is formed by a compatibility treatment of modified silica powder and fluorinated polyacrylate emulsion to form a stable mesh crosslinking structure.

Benefits of technology

It significantly improves the waterproof performance, aging resistance, flexibility, adhesion, wear resistance and chemical corrosion resistance of waterproof coatings, extends its service life, and shows good stability and weather resistance in mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof coatings, in particular to a cement waterproof coating based on a polymer and a preparation process of the cement waterproof coating. Linear silicon dioxide is prepared by taking ammonia water and tetraethoxysilane as raw materials and is coated with dopamine hydrochloride and trihydroxymethyl aminomethane; nanospheres generated by tetraethoxysilane are deposited on the surface of linear silicon dioxide, so that the prepared modified silicon dioxide powder is better compatible with a fluorinated polyacrylate emulsion, the mechanical property of a waterproof coating film is improved by adding the modified silicon dioxide powder, and the adhesive force of the waterproof coating on the surface of cement is improved; the filler component and the modified silicon dioxide powder are treated by the coupling agent and then added into the fluorinated polyacrylate emulsion, so that the compatibility of the filler component and the modified silicon dioxide powder of the powder with the fluorinated polyacrylate emulsion can be improved, and the prepared waterproof coating has stable wear resistance and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coatings, and in particular to a polymer-based cement waterproof coating and a preparation process thereof. Background Art

[0002] In the construction industry, waterproof coatings are key materials for protecting buildings from water erosion, and their performance directly affects the service life and safety of buildings. With the continuous advancement of construction technology and the improvement of people's requirements for building quality, waterproof coatings need to have not only good waterproof performance, but also excellent mechanical properties to cope with challenges in various complex environments and use conditions. Although traditional waterproof materials, such as asphalt and rubber, can meet the waterproofing needs to a certain extent, they often have disadvantages such as easy aging, easy cracking, and poor mechanical properties, which make it difficult to meet the high standards of modern buildings for waterproof materials.

[0003] Waterproof coatings need to be able to effectively prevent water penetration and protect building structures and internal facilities from water damage. Polymer-based cement waterproof coatings form a dense waterproof film layer by compounding polymer emulsions with inorganic materials such as cement, which effectively prevents water penetration. However, the waterproof performance of some waterproof coatings in the prior art may decrease after long-term immersion or extreme climatic conditions, resulting in waterproof failure. Therefore, how to improve the waterproof performance of waterproof coatings, especially their long-term water resistance, has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention

[0004] Technical issues solved In view of the above-mentioned shortcomings of the prior art, the present invention provides a polymer-based cement waterproof coating and a preparation process thereof, which can effectively solve the problem that the waterproof performance of the cement waterproof coating in the prior art cannot meet the industry demand.

[0005] Technical Solution To achieve the above objectives, the present invention is implemented through the following technical solutions: A polymer-based cement waterproof coating, the polymer-based cement waterproof coating consisting of the following components: fluoropolyacrylate emulsion, modified silica powder, filler component, coupling agent, defoamer, water reducing agent, composite curing agent component and deionized water; The fluoropolyacrylate emulsion is prepared by emulsion polymerization using perfluoroalkylethyl acrylate, octadecyl methacrylate, hydroxypropyl acrylate and p-chloromethylstyrene as raw materials; The modified silicon dioxide powder is prepared using tetraethyl orthosilicate and dopamine hydrochloride as raw materials; The filler component is prepared by taking precipitated barium sulfate, heavy calcium carbonate, quartz powder and kaolin as raw materials.

[0006] Furthermore, the preparation method of the fluorinated polyacrylate emulsion is: S2.1. Weigh 1 g of ammonium persulfate and dissolve it in 20 g of deionized water. Stir and dissolve the resulting solution as the ammonium persulfate aqueous solution. S2.2. Weigh 1g of sodium dodecyl sulfate, 2g of fatty alcohol polyoxyethylene ether and 50g of deionized water into a flask, stir and heat to 70-80°C, and under nitrogen protection, drop 27g of perfluoroalkylethyl acrylate, 17g of octadecyl methacrylate, 1.5g of hydroxypropyl acrylate, 2g of p-chloromethylstyrene and 21g of aqueous ammonium persulfate solution, react at 75-85°C for 3-4h and then cool to room temperature to obtain a fluoropolyacrylate emulsion.

[0007] Furthermore, the specific operation of stirring and dissolving in S2.1 is stirring at a speed of 500 r / min for 10 min, the speed of stirring and heating in S2.2 is 300 r / min, and the dripping rate in S2.2 is 1 drop / s.

[0008] Furthermore, the preparation method of the modified silicon dioxide powder is: S4.1. Add 5 mL of ethyl orthosilicate to 50 mL of 90% ethanol aqueous solution, adjust the pH to 9 with ammonia water, and stir at room temperature for 20 min. Then, heat to 35°C and age for 2 h. Finally, dry in an oven at 80°C to constant weight. The obtained product is recorded as spherical silica. S4.2, weigh 16g of polyvinyl pyrrolidone and add it to 160mL of n-pentanol, stir evenly and oscillate ultrasonically for 2h, then add 15mL of ethanol and 5mL of deionized water and shake by hand for 3min, drop 1.6mL of 0.18mol / L sodium citrate dihydrate aqueous solution, continue to shake by hand for 3min, then drop 3mL of ammonia water and let stand for 5min, finally drop 1.5mL of tetraethyl orthosilicate and shake by hand again for 3min, the result is recorded as the reaction system; S4.3, the reaction system was sealed and placed in an oil bath at 90°C for 180 min, followed by filtration using a polytetrafluoroethylene membrane with a pore size of 0.45 μm. The obtained product was washed with anhydrous ethanol and deionized water three times each, and then dried in an oven at 80°C for 2 h. The obtained product was recorded as linear silica; S4.4. Pour 1g of linear silica, 10mL of anhydrous ethanol and 3mL of deionized water into a flask, add 0.11g of dopamine hydrochloride and then add tris(hydroxymethyl)aminomethane to adjust the pH value to 8.5, then add 1mL of ethyl orthosilicate and let stand in an oil bath at 30°C for 24h, filter with a polytetrafluoroethylene membrane with a pore size of 0.45μm, wash with anhydrous ethanol and deionized water three times each and dry in an oven at 80°C for 2h, and grind through a 200-mesh sieve to obtain modified silica powder.

[0009] Furthermore, the rotation speed of the stirring reaction in S4.1 is 300 r / min, the uniform stirring operation in S4.2 is stirring at a rotation speed of 500 r / min for 10 min, the dripping rate in S4.2 is 1 drop / s, the power of ultrasonic oscillation in S4.2 is 200 W, and the dripping rate in S4.4 is 1 drop / s.

[0010] Furthermore, the preparation method of the filler component is: weigh 1250 mesh precipitated barium sulfate, 800 mesh heavy calcium carbonate, 1200 mesh quartz powder and 800 mesh kaolin in a weight ratio of 2:1:2:1, pour them into a ball mill for ball milling and mixing, and the result is the filler component.

[0011] Furthermore, the coupling agent is silane coupling agent KH-550, the defoaming agent is polyether modified silicon defoaming agent, and the water reducing agent is polycarboxylic acid water reducing agent.

[0012] Furthermore, the composite curing agent component is prepared by mixing an epoxy curing agent and an isocyanate curing agent in an equal weight ratio.

[0013] A preparation process of a polymer-based cement waterproof coating, the preparation process comprising the following steps: Step 1, weighing 15-20 parts by weight of modified silica powder, 15-18 parts by weight of filler component, 2-3 parts by weight of coupling agent and 8-10 parts by weight of deionized water into a ball mill for ball milling and mixing, and the obtained solid component is recorded; Step 2, weigh 28-30 parts by weight of solid components, 1-2 parts by weight of defoamer, 1-2 parts by weight of water reducer and 35-40 parts by weight of deionized water, pour into the dispersant for mixing and dispersion, add 80-100 parts by weight of fluoropolyacrylate emulsion under stirring conditions after passing through a 100-mesh sieve, stir at the original stirring speed for 30 minutes, then add 1-2 parts by weight of the composite curing agent component, continue stirring for 10 minutes to obtain a polymer-based cement waterproof coating.

[0014] Furthermore, the rotation speed of the ball milling mixing in step 1 is 800 r / min, the specific operation of the mixing and dispersing in step 2 is stirring at a rotation speed of 500 r / min for 10 minutes, and the rotation speed of the stirring condition in step 2 is 300 r / min.

[0015] Beneficial Effects The present invention provides a polymer-based cement waterproof coating and a preparation process thereof. Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses perfluoroalkyl ethyl acrylate, octadecyl methacrylate, hydroxypropyl acrylate and p-chloromethylstyrene as raw materials to prepare fluorinated polyacrylate emulsion through emulsion polymerization. Using fluorinated polyacrylate emulsion as the base liquid of waterproof coating can make the prepared waterproof coating have excellent waterproof performance. Perfluoroalkyl ethyl acrylate is used as a key monomer, and its long-chain fluoroalkyl group has extremely low surface energy, which can effectively reduce the surface tension of the coating film, making it difficult for water to adhere to and penetrate the surface of the coating film, thereby significantly improving the waterproof performance of the coating. Moreover, the monomers can be formed into a dense copolymer through emulsion polymerization, further enhancing the waterproof barrier effect of the coating film; secondly, the fluorinated polyacrylate emulsion has excellent chemical stability and can The invention can resist the erosion of natural factors such as ultraviolet rays, temperature changes, wind and rain, so as to maintain the stability of the coating film, while the octadecyl methacrylate and parachloromethylstyrene in the copolymer can improve the aging resistance of the coating, making it less likely to yellow and crack during use, thereby increasing the effective service life of the waterproof coating to a certain extent; the invention uses the above four monomers as raw materials to prepare the fluoropolyacrylate emulsion, and can combine the properties of each monomer to make the prepared cement waterproof coating have excellent waterproof effect, and also have good flexibility, adhesion, wear resistance, weather resistance, chemical corrosion resistance and other comprehensive properties, and can give full play to the outstanding performance of different monomers, thereby improving the performance of the prepared waterproof coating as a whole.

[0016] 2. The present invention uses ammonia water and tetraethyl orthosilicate as raw materials to prepare linear silica, and then coats the linear silica with dopamine hydrochloride and trishydroxymethylaminomethane, and then uses tetraethyl orthosilicate to generate nanospheres and deposit them on the surface of the linear silica, so that the prepared modified silica powder can be better compatible with the fluoropolyacrylate emulsion, and the addition of the modified silica powder can improve the mechanical properties of the waterproof coating film and improve the adhesion of the waterproof coating on the cement surface; secondly, the filler component and the modified silica powder are treated with a coupling agent and then added to the fluoropolyacrylate emulsion, which can improve the compatibility of the filler component of the powder and the modified silica powder with the fluoropolyacrylate emulsion. Compatibility: Since a large number of nanospheres are precipitated on the surface of the modified silica powder prepared in the present invention, these nanospheres can be combined with the silane coupling agent through hydrogen bonding. Therefore, when the modified silica powder is mixed into the fluoropolyacrylate emulsion, the modified silica powder and the fluoropolyacrylate emulsion can be combined through hydrogen bonding to form a stable network cross-linked structure, and the filler component can be evenly dispersed in the gaps of the network cross-linked structure to form a stable waterproof structure. Moreover, the modified silica powder and the filler component are both wear-resistant powders. Through the effect of the above-mentioned network structure, the prepared waterproof coating can have stable wear resistance in addition to having a good waterproof effect. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] The present invention will be further described below in conjunction with the embodiments.

[0019] Example 1 A polymer-based cement waterproof coating of this embodiment, the polymer-based cement waterproof coating is composed of the following components: fluoropolyacrylate emulsion, modified silica powder, filler component, coupling agent, defoamer, water reducing agent, composite curing agent component and deionized water; The fluorinated polyacrylate emulsion is prepared by emulsion polymerization using perfluoroalkyl ethyl acrylate, octadecyl methacrylate, hydroxypropyl acrylate and p-chloromethylstyrene as raw materials, wherein the preparation method of the fluorinated polyacrylate emulsion is as follows: S2.1. Weigh 1 g of ammonium persulfate and dissolve it in 20 g of deionized water. Stir at 500 r / min for 10 min and the resulting solution is recorded as the ammonium persulfate aqueous solution. S2.2. Weigh 1g of sodium dodecyl sulfate, 2g of fatty alcohol polyoxyethylene ether and 50g of deionized water into a flask, stir at a speed of 300r / min, heat to 70°C, and under nitrogen protection, drop 27g of perfluoroalkylethyl acrylate, 17g of octadecyl methacrylate, 1.5g of hydroxypropyl acrylate, 2g of p-chloromethylstyrene and 21g of ammonium persulfate aqueous solution at a drop rate of 1 drop / s. React at 75°C for 3h and then cool to room temperature to obtain a fluoropolyacrylate emulsion.

[0020] The modified silicon dioxide powder is prepared with tetraethyl orthosilicate and dopamine hydrochloride as raw materials, wherein the preparation method of the modified silicon dioxide powder is as follows: S4.1. Add 5 mL of ethyl orthosilicate to 50 mL of 90% ethanol aqueous solution, adjust the pH to 9 with ammonia water, stir at 300 r / min at room temperature for 20 min, then heat to 35°C and age for 2 h, finally dry in an oven at 80°C to constant weight, the result is recorded as spherical silica; S4.2, weigh 16g of polyvinyl pyrrolidone and add it to 160mL of n-pentanol, stir at a speed of 500r / min for 10min, then ultrasonically oscillate at a power of 200W for 2h, then add 15mL of ethanol and 5mL of deionized water and shake by hand for 3min, drop 1.6mL of 0.18mol / L sodium citrate dihydrate aqueous solution at a drop rate of 1 drop / s, continue to shake by hand for 3min, then drop 3mL of ammonia water at a drop rate of 1 drop / s and let stand for 5min, finally drop 1.5mL of tetraethyl orthosilicate at a drop rate of 1 drop / s and shake by hand again for 3min, the result is recorded as the reaction system; S4.3, the reaction system was sealed and placed in an oil bath at 90°C for 180 min, followed by filtration using a polytetrafluoroethylene membrane with a pore size of 0.45 μm. The obtained product was washed with anhydrous ethanol and deionized water three times each, and then dried in an oven at 80°C for 2 h. The obtained product was recorded as linear silica; S4.4. Pour 1g of linear silica, 10mL of anhydrous ethanol and 3mL of deionized water into a flask, add 0.11g of dopamine hydrochloride, then add tris(hydroxymethyl)aminomethane at a rate of 1 drop / s to adjust the pH value to 8.5, then add 1mL of ethyl orthosilicate and let stand in an oil bath at 30°C for 24h. After filtering with a polytetrafluoroethylene membrane with a pore size of 0.45μm, wash with anhydrous ethanol and deionized water 3 times each and dry in an oven at 80°C for 2h. Grind through a 200-mesh sieve to obtain modified silica powder.

[0021] The filler component is prepared with precipitated barium sulfate, heavy calcium carbonate, quartz powder and kaolin as raw materials, wherein the preparation method of the filler component is: weigh 1250 mesh precipitated barium sulfate, 800 mesh heavy calcium carbonate, 1200 mesh quartz powder and 800 mesh kaolin in a weight ratio of 2:1:2:1, pour them into a ball mill for ball milling and mixing, and the result is the filler component.

[0022] The coupling agent is silane coupling agent KH-550, the defoaming agent is polyether modified silicon defoaming agent, and the water reducing agent is polycarboxylic acid water reducing agent.

[0023] The composite curing agent component is prepared by mixing an epoxy curing agent and an isocyanate curing agent in an equal weight ratio.

[0024] A preparation process of a polymer-based cement waterproof coating, the preparation process comprising the following steps: Step 1, weighing 15 parts by weight of modified silica powder, 15 parts by weight of filler component, 2 parts by weight of coupling agent and 8 parts by weight of deionized water, pouring them into a ball mill and mixing them at a speed of 800 r / min, and the obtained solid component is recorded; Step 2: Weigh 28 parts by weight of solid components, 1 part by weight of defoamer, 1 part by weight of water reducer and 35 parts by weight of deionized water into the dispersant and stir at a speed of 500 r / min for 10 minutes. After passing through a 100-mesh sieve, add 80 parts by weight of fluoropolyacrylate emulsion at a stirring speed of 300 r / min. After stirring at the original stirring speed for 30 minutes, add 1 part by weight of the composite curing agent component, and continue stirring for 10 minutes to obtain a polymer-based cement waterproof coating.

[0025] Example 2 A polymer-based cement waterproof coating of this embodiment, the polymer-based cement waterproof coating is composed of the following components: fluoropolyacrylate emulsion, modified silica powder, filler component, coupling agent, defoamer, water reducing agent, composite curing agent component and deionized water; The fluorinated polyacrylate emulsion is prepared by emulsion polymerization using perfluoroalkyl ethyl acrylate, octadecyl methacrylate, hydroxypropyl acrylate and p-chloromethylstyrene as raw materials, wherein the preparation method of the fluorinated polyacrylate emulsion is as follows: S2.1. Weigh 1 g of ammonium persulfate and dissolve it in 20 g of deionized water. Stir at 500 r / min for 10 min and the resulting solution is recorded as the ammonium persulfate aqueous solution. S2.2. Weigh 1g of sodium dodecyl sulfate, 2g of fatty alcohol polyoxyethylene ether and 50g of deionized water into a flask, stir at a speed of 300r / min, heat to 80°C, and under nitrogen protection, drop 27g of perfluoroalkylethyl acrylate, 17g of octadecyl methacrylate, 1.5g of hydroxypropyl acrylate, 2g of p-chloromethylstyrene and 21g of ammonium persulfate aqueous solution at a drop rate of 1 drop / s. React at 85°C for 4h and then cool to room temperature to obtain a fluoropolyacrylate emulsion.

[0026] The modified silicon dioxide powder is prepared with tetraethyl orthosilicate and dopamine hydrochloride as raw materials, wherein the preparation method of the modified silicon dioxide powder is as follows: S4.1. Add 5 mL of ethyl orthosilicate to 50 mL of 90% ethanol aqueous solution, adjust the pH to 9 with ammonia water, stir at 300 r / min at room temperature for 20 min, then heat to 35°C and age for 2 h, finally dry in an oven at 80°C to constant weight, the result is recorded as spherical silica; S4.2, weigh 16g of polyvinyl pyrrolidone and add it to 160mL of n-pentanol, stir at a speed of 500r / min for 10min, then ultrasonically oscillate at a power of 200W for 2h, then add 15mL of ethanol and 5mL of deionized water and shake by hand for 3min, drop 1.6mL of 0.18mol / L sodium citrate dihydrate aqueous solution at a drop rate of 1 drop / s, continue to shake by hand for 3min, then drop 3mL of ammonia water at a drop rate of 1 drop / s and let stand for 5min, finally drop 1.5mL of tetraethyl orthosilicate at a drop rate of 1 drop / s and shake by hand again for 3min, the result is recorded as the reaction system; S4.3, the reaction system was sealed and placed in an oil bath at 90°C for 180 min, followed by filtration using a polytetrafluoroethylene membrane with a pore size of 0.45 μm. The obtained product was washed with anhydrous ethanol and deionized water three times each, and then dried in an oven at 80°C for 2 h. The obtained product was recorded as linear silica; S4.4. Pour 1g of linear silica, 10mL of anhydrous ethanol and 3mL of deionized water into a flask, add 0.11g of dopamine hydrochloride, then add tris(hydroxymethyl)aminomethane at a rate of 1 drop / s to adjust the pH value to 8.5, then add 1mL of ethyl orthosilicate and let stand in an oil bath at 30°C for 24h. After filtering with a polytetrafluoroethylene membrane with a pore size of 0.45μm, wash with anhydrous ethanol and deionized water 3 times each and dry in an oven at 80°C for 2h. Grind through a 200-mesh sieve to obtain modified silica powder.

[0027] The filler component is prepared with precipitated barium sulfate, heavy calcium carbonate, quartz powder and kaolin as raw materials, wherein the preparation method of the filler component is: weigh 1250 mesh precipitated barium sulfate, 800 mesh heavy calcium carbonate, 1200 mesh quartz powder and 800 mesh kaolin in a weight ratio of 2:1:2:1, pour them into a ball mill for ball milling and mixing, and the result is the filler component.

[0028] The coupling agent is silane coupling agent KH-550, the defoaming agent is polyether modified silicon defoaming agent, and the water reducing agent is polycarboxylic acid water reducing agent.

[0029] The composite curing agent component is prepared by mixing an epoxy curing agent and an isocyanate curing agent in an equal weight ratio.

[0030] A preparation process of a polymer-based cement waterproof coating, the preparation process comprising the following steps: Step 1, weighing 20 parts by weight of modified silica powder, 18 parts by weight of filler component, 3 parts by weight of coupling agent and 10 parts by weight of deionized water into a ball mill and mixing them at a speed of 800 r / min, and the obtained solid component is recorded; Step 2: weigh 30 parts by weight of solid components, 2 parts by weight of defoamer, 2 parts by weight of water reducer and 40 parts by weight of deionized water, pour them into the dispersant and stir at a speed of 500 r / min for 10 minutes. After passing through a 100-mesh sieve, add 100 parts by weight of fluoropolyacrylate emulsion under stirring conditions at a speed of 300 r / min. After stirring at the original stirring speed for 30 minutes, add 2 parts by weight of composite curing agent component, and continue stirring for 10 minutes to obtain a polymer-based cement waterproof coating.

[0031] Example 3 A polymer-based cement waterproof coating of this embodiment, the polymer-based cement waterproof coating is composed of the following components: fluoropolyacrylate emulsion, modified silica powder, filler component, coupling agent, defoamer, water reducing agent, composite curing agent component and deionized water; The fluorinated polyacrylate emulsion is prepared by emulsion polymerization using perfluoroalkyl ethyl acrylate, octadecyl methacrylate, hydroxypropyl acrylate and p-chloromethylstyrene as raw materials, wherein the preparation method of the fluorinated polyacrylate emulsion is as follows: S2.1. Weigh 1 g of ammonium persulfate and dissolve it in 20 g of deionized water. Stir at 500 r / min for 10 min and the resulting solution is recorded as the ammonium persulfate aqueous solution. S2.2. Weigh 1g of sodium dodecyl sulfate, 2g of fatty alcohol polyoxyethylene ether and 50g of deionized water into a flask, stir at a speed of 300r / min, heat to 75°C, and under nitrogen protection, drop 27g of perfluoroalkylethyl acrylate, 17g of octadecyl methacrylate, 1.5g of hydroxypropyl acrylate, 2g of p-chloromethylstyrene and 21g of ammonium persulfate aqueous solution at a drop rate of 1 drop / s. React at 80°C for 4h and then cool to room temperature to obtain a fluoropolyacrylate emulsion.

[0032] The modified silicon dioxide powder is prepared with tetraethyl orthosilicate and dopamine hydrochloride as raw materials, wherein the preparation method of the modified silicon dioxide powder is as follows: S4.1. Add 5 mL of ethyl orthosilicate to 50 mL of 90% ethanol aqueous solution, adjust the pH to 9 with ammonia water, stir at 300 r / min at room temperature for 20 min, then heat to 35°C and age for 2 h, finally dry in an oven at 80°C to constant weight, the result is recorded as spherical silica; S4.2, weigh 16g of polyvinyl pyrrolidone and add it to 160mL of n-pentanol, stir at a speed of 500r / min for 10min, then ultrasonically oscillate at a power of 200W for 2h, then add 15mL of ethanol and 5mL of deionized water and shake by hand for 3min, drop 1.6mL of 0.18mol / L sodium citrate dihydrate aqueous solution at a drop rate of 1 drop / s, continue to shake by hand for 3min, then drop 3mL of ammonia water at a drop rate of 1 drop / s and let stand for 5min, finally drop 1.5mL of tetraethyl orthosilicate at a drop rate of 1 drop / s and shake by hand again for 3min, the result is recorded as the reaction system; S4.3, the reaction system was sealed and placed in an oil bath at 90°C for 180 min, followed by filtration using a polytetrafluoroethylene membrane with a pore size of 0.45 μm. The obtained product was washed with anhydrous ethanol and deionized water three times each, and then dried in an oven at 80°C for 2 h. The obtained product was recorded as linear silica; S4.4. Pour 1g of linear silica, 10mL of anhydrous ethanol and 3mL of deionized water into a flask, add 0.11g of dopamine hydrochloride, then add tris(hydroxymethyl)aminomethane at a rate of 1 drop / s to adjust the pH value to 8.5, then add 1mL of ethyl orthosilicate and let stand in an oil bath at 30°C for 24h. After filtering with a polytetrafluoroethylene membrane with a pore size of 0.45μm, wash with anhydrous ethanol and deionized water 3 times each and dry in an oven at 80°C for 2h. Grind through a 200-mesh sieve to obtain modified silica powder.

[0033] The filler component is prepared with precipitated barium sulfate, heavy calcium carbonate, quartz powder and kaolin as raw materials, wherein the preparation method of the filler component is: weigh 1250 mesh precipitated barium sulfate, 800 mesh heavy calcium carbonate, 1200 mesh quartz powder and 800 mesh kaolin in a weight ratio of 2:1:2:1, pour them into a ball mill for ball milling and mixing, and the result is the filler component.

[0034] The coupling agent is silane coupling agent KH-550, the defoaming agent is polyether modified silicon defoaming agent, and the water reducing agent is polycarboxylic acid water reducing agent.

[0035] The composite curing agent component is prepared by mixing an epoxy curing agent and an isocyanate curing agent in an equal weight ratio.

[0036] A preparation process of a polymer-based cement waterproof coating, the preparation process comprising the following steps: Step 1, weighing 18 parts by weight of modified silica powder, 17 parts by weight of filler component, 3 parts by weight of coupling agent and 9 parts by weight of deionized water into a ball mill and mixing them at a speed of 800 r / min, and the obtained solid component is recorded; Step 2: Weigh 29 parts by weight of solid components, 2 parts by weight of defoamer, 2 parts by weight of water reducer and 38 parts by weight of deionized water into the dispersant and stir at a speed of 500 r / min for 10 minutes. After passing through a 100-mesh sieve, add 90 parts by weight of fluoropolyacrylate emulsion at a stirring speed of 300 r / min. After stirring at the original stirring speed for 30 minutes, add 2 parts by weight of composite curing agent component, and continue stirring for 10 minutes to obtain a polymer-based cement waterproof coating.

[0037] Comparative Example 1 The polymer-based cement waterproof coating and its preparation process provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the modified silica powder in Example 1 is replaced with nano-silicon dioxide.

[0038] Comparative Example 2 The polymer-based cement waterproof coating and its preparation process provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 2, the filler component in Example 1 is replaced with 1250 mesh precipitated barium sulfate.

[0039] Comparative Example 3 The polymer-based cement waterproof coating and its preparation process provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 3, the filler component in Example 1 is replaced with 1200 mesh quartz powder.

[0040] Comparative Example 4 The polymer-based cement waterproof coating and its preparation process provided in this comparative example are roughly the same as those in Example 1, with the main difference being that in this comparative example 4, the weight ratio of precipitated barium sulfate, heavy calcium carbonate, quartz powder and kaolin in Example 1 is replaced with 1:2:1:2.

[0041] Comparative Example 5 The polymer-based cement waterproof coating and its preparation process provided in this comparative example are roughly the same as those in Example 1, with the main difference being that the steps of the preparation process of the polymer-based cement waterproof coating in Example 1 are modified in this comparative example 5 as follows: Step 1, weighing 18 parts by weight of modified silica powder, 12 parts by weight of filler component, 1 part by weight of coupling agent and 8 parts by weight of deionized water into a ball mill and mixing them at a speed of 800 r / min, and the obtained mixture is recorded as a solid component; Step 2: weigh 25 parts by weight of solid components, 2 parts by weight of defoamer, 2 parts by weight of water reducer and 32 parts by weight of deionized water, pour them into the dispersant and stir at a speed of 500 r / min for 10 minutes. After passing through a 100-mesh sieve, add 90 parts by weight of fluoropolyacrylate emulsion under stirring conditions at a speed of 300 r / min. After stirring at the original stirring speed for 30 minutes, add 2 parts by weight of composite curing agent component, and continue stirring for 10 minutes to obtain a polymer-based cement waterproof coating.

[0042] Performance Testing The polymer-based cement waterproof coatings in Examples 1-3 and Comparative Examples 1-5 are marked as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5, respectively. Then, the performance of Examples 1-3 and Comparative Examples 1-5 is tested. The specific testing methods and test items are as follows: 1. The polymer-based cement waterproof coatings of Examples 1-3 and Comparative Examples 1-5 were applied into coatings, and then their contact angles were measured respectively. The obtained data were recorded in the following table; 2. The tensile properties of the polymer-based cement waterproof coatings of Examples 1-3 and Comparative Examples 1-5 were tested with reference to GB / T16777-2008 "Test Methods for Building Waterproof Coatings", and the obtained data are recorded in the following table; 3. The pencil hardness of the polymer-based cement waterproof coatings of Examples 1-3 and Comparative Examples 1-5 was tested according to GB / T6739-2006 "Determination of paint film hardness by pencil method for paints and varnishes", and the obtained data are recorded in the following table; 4. The film layers coated with the polymer-based cement waterproof coatings of Examples 1-3 and Comparative Examples 1-5 were subjected to friction and wear tests using an MFT-5000 friction and wear testing machine with a reciprocating distance of 4 mm, an operating frequency of 200 times / min, a rated load of 2.2 N, a test time of 30 min, and the wear amount was calculated. The obtained wear rate data are recorded in the table below.

[0043]

[0044] It can be seen from the data in the above table that the contact angle of the polymer-based cement waterproof coating in the present embodiments 1-3 is relatively large, indicating that the polymer-based cement waterproof coating in the present embodiments 1-3 has excellent waterproof performance; compared with comparative example 1, the polymer-based cement waterproof coating in the present embodiments 1-3 has a significantly lower wear rate, indicating that the modified silica powder added to the cement waterproof coating can improve the wear resistance of the coating.

[0045] Secondly, the polymer-based cement waterproof coatings in Examples 1-3 have higher pencil hardness and stronger tensile strength than those in Comparative Examples 2-3, indicating that the filler component after multi-component mixing is more capable of improving the mechanical properties of the coating than the single-component 1250 mesh precipitated barium sulfate or 1200 mesh quartz powder; and the polymer-based cement waterproof coatings in Examples 1-3 have higher pencil hardness, tensile strength and lower wear rate than Comparative Example 4, indicating that the filler component prepared by mixing precipitated barium sulfate, heavy calcium carbonate, quartz powder and kaolin in the mass ratio of the present invention can assist the coating to have better mechanical properties and wear resistance.

[0046] Compared with Comparative Example 5, the overall performance of the polymer-based cement waterproof coating in Examples 1-3 is significantly better. This is because Comparative Example 5 reduces the amount of filler components, and the filler components are wear-resistant components that can improve the wear resistance and mechanical properties of the coating. Too low an amount added will reduce the hardness and wear resistance of the coating. The weight ratio of the ingredients in Examples 1-3 is more appropriate, which can make the prepared water-based paint coating have better wear resistance. This shows that a polymer-based cement waterproof coating prepared by the preparation process of the present invention has better market application prospects.

[0047] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0048] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A polymer-based cement waterproof coating, characterized in that: The polymer-based cement waterproof coating is composed of the following components: fluoropolyacrylate emulsion, modified silica powder, filler component, coupling agent, defoamer, water reducing agent, composite curing agent component and deionized water; The fluorinated polyacrylate emulsion is prepared by emulsion polymerization using perfluoroalkylethyl acrylate, octadecyl methacrylate, hydroxypropyl acrylate and p-chloromethylstyrene as raw materials; The modified silicon dioxide powder is prepared using tetraethyl orthosilicate and dopamine hydrochloride as raw materials; The filler component is prepared by taking precipitated barium sulfate, heavy calcium carbonate, quartz powder and kaolin as raw materials.

2. A polymer-based cement waterproof coating according to claim 1, characterized in that: The preparation method of the fluorinated polyacrylate emulsion is: S2.

1. Weigh 1 g of ammonium persulfate and dissolve it in 20 g of deionized water. Stir and dissolve the resulting solution as the ammonium persulfate aqueous solution. S2.

2. Weigh 1g of sodium dodecyl sulfate, 2g of fatty alcohol polyoxyethylene ether and 50g of deionized water into a flask, stir and heat to 70-80°C, and under nitrogen protection, drop 27g of perfluoroalkylethyl acrylate, 17g of octadecyl methacrylate, 1.5g of hydroxypropyl acrylate, 2g of p-chloromethylstyrene and 21g of aqueous ammonium persulfate solution, react at 75-85°C for 3-4h and then cool to room temperature to obtain a fluoropolyacrylate emulsion.

3. A polymer-based cement waterproof coating according to claim 2, characterized in that: The specific operation of stirring and dissolving in S2.1 is stirring at a speed of 500 r / min for 10 min, the speed of stirring and heating in S2.2 is 300 r / min, and the dripping rate in S2.2 is 1 drop / s.

4. A polymer-based cement waterproof coating according to claim 1, characterized in that: The preparation method of the modified silicon dioxide powder is: S4.

1. Add 5 mL of ethyl orthosilicate to 50 mL of 90% ethanol aqueous solution, adjust the pH to 9 with ammonia water, and stir at room temperature for 20 min. Then, heat to 35°C and age for 2 h. Finally, dry in an oven at 80°C to constant weight. The obtained product is recorded as spherical silica. S4.2, weigh 16g of polyvinyl pyrrolidone and add it to 160mL of n-pentanol, stir evenly and oscillate ultrasonically for 2h, then add 15mL of ethanol and 5mL of deionized water and shake by hand for 3min, drop 1.6mL of 0.18mol / L sodium citrate dihydrate aqueous solution, continue to shake by hand for 3min, then drop 3mL of ammonia water and let stand for 5min, finally drop 1.5mL of tetraethyl orthosilicate and shake by hand again for 3min, the result is recorded as the reaction system; S4.3, the reaction system was sealed and placed in an oil bath at 90°C for 180 min, followed by filtration using a polytetrafluoroethylene membrane with a pore size of 0.45 μm. The obtained product was washed with anhydrous ethanol and deionized water three times each, and then dried in an oven at 80°C for 2 h. The obtained product was recorded as linear silica; S4.

4. Pour 1g of linear silica, 10mL of anhydrous ethanol and 3mL of deionized water into a flask, add 0.11g of dopamine hydrochloride and then add tris(hydroxymethyl)aminomethane to adjust the pH value to 8.5, then add 1mL of ethyl orthosilicate and let stand in an oil bath at 30°C for 24h, filter with a polytetrafluoroethylene membrane with a pore size of 0.45μm, wash with anhydrous ethanol and deionized water three times each and dry in an oven at 80°C for 2h, and grind through a 200-mesh sieve to obtain modified silica powder.

5. A polymer-based cement waterproof coating according to claim 4, characterized in that: The speed of the stirring reaction in S4.1 is 300 r / min, the uniform stirring operation in S4.2 is stirring at a speed of 500 r / min for 10 min, the dripping rate in S4.2 is 1 drop / s, the power of the ultrasonic oscillation in S4.2 is 200 W, and the dripping rate in S4.4 is 1 drop / s.

6. A polymer-based cement waterproof coating according to claim 1, characterized in that: The preparation method of the filler component is as follows: weigh 1250-mesh precipitated barium sulfate, 800-mesh heavy calcium carbonate, 1200-mesh quartz powder and 800-mesh kaolin in a weight ratio of 2:1:2:1, pour them into a ball mill for ball milling and mixing, and the obtained filler component is obtained.

7. A polymer-based cement waterproof coating according to claim 1, characterized in that: The coupling agent is silane coupling agent KH-550, the defoamer is polyether modified silicon defoamer, and the water reducer is polycarboxylic acid water reducer.

8. The polymer-based cement waterproof coating according to claim 1, characterized in that: The composite curing agent component is prepared by mixing an epoxy curing agent and an isocyanate curing agent in an equal weight ratio.

9. A process for preparing a polymer-based cement waterproof coating according to any one of claims 1 to 8, characterized in that: The preparation process comprises the following steps: Step 1, weighing 15-20 parts by weight of modified silica powder, 15-18 parts by weight of filler component, 2-3 parts by weight of coupling agent and 8-10 parts by weight of deionized water into a ball mill for ball milling and mixing, and the obtained solid component is recorded; Step 2, weigh 28-30 parts by weight of solid components, 1-2 parts by weight of defoamer, 1-2 parts by weight of water reducer and 35-40 parts by weight of deionized water, pour into the dispersant for mixing and dispersion, add 80-100 parts by weight of fluoropolyacrylate emulsion under stirring conditions after passing through a 100-mesh sieve, stir at the original stirring speed for 30 minutes, then add 1-2 parts by weight of the composite curing agent component, continue stirring for 10 minutes to obtain a polymer-based cement waterproof coating.

10. The preparation process of a polymer-based cement waterproof coating according to claim 9, characterized in that: The rotation speed of the ball milling mixing in step 1 is 800 r / min, and the specific operation of the mixing and dispersing in step 2 is stirring at a rotation speed of 500 r / min for 10 min. The rotation speed of the stirring condition in step 2 is 300 r / min.

Citation Information

Patent Citations

  • Preparation method of (sesqui) siloxane hybrid modified fluorinated polyacrylate emulsion

    CN102443099A

  • Waterproof coating material for garden road and construction method thereof

    CN109762428A

  • Waterproof coating and preparation method thereof

    CN112322135A

  • Modified epoxy resin, preparation method of modified epoxy resin, emulsion preparation method of modified epoxy resin and application thereof

    CN113004494A

  • Preparation method of wear-resistant powder with high transparency

    CN114180587A