Coating as well as preparation method and application thereof

By blending two types of polyaspartic ester resins and using IPDI aliphatic isocyanate prepolymer, a highly rain-resistant leading edge protective coating for wind turbine blades was prepared. This solved the problem of insufficient protection of traditional coatings in rain-eroded environments and improved the operating efficiency and environmental friendliness of wind turbine units.

CN118931341APending Publication Date: 2024-11-12TIANJIN BEACON PAINTING MATERIALS CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411146606.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional wind turbine blade leading edge protective coatings cannot provide long-term protection in high-intensity rain erosion environments, leading to a decrease in the operating efficiency of wind turbine units.

Method used

A coating with ultra-high elongation and tensile strength was prepared by blending two polyaspartic ester resins and using an IPDI-based aliphatic isocyanate prepolymer, ensuring excellent rain erosion resistance at low temperatures.

Benefits of technology

It offers superior resistance to rain erosion and physicochemical properties, while ensuring the coating's workability. It is also free of heavy metals, making it more environmentally friendly and safer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003047570000091
    Figure BDA0005003047570000091
  • Figure BDA0005003047570000101
    Figure BDA0005003047570000101
Patent Text Reader

Abstract

The invention relates to a coating as well as a preparation method and application thereof. The coating is prepared from a first component and a second component, the first component and the second component are matched according to the NCO / NH ratio of 0.8-1.1, and the first component is prepared from 15-25 parts of polyaspartic acid ester resin A, 15-25 parts of polyaspartic acid ester resin B, 0.5-1.5 parts of a dispersing agent, 1-3 parts of a defoaming agent, 1-4 parts of a water absorbent, 0.5-1 part of a flatting agent, 0.2-1 part of a thixotropic additive and 1-3 parts of a light absorber; the total content of the polyaspartic acid ester resin A and the polyaspartic acid ester resin B is controlled to be 40 parts, and the total content of the polyaspartic acid ester resin A and the polyaspartic acid ester resin B is controlled to be 40 parts. And the component II is prepared from 100 parts of an aliphatic isocyanate prepolymer based on IPDI (isophorone diisocyanate). The coating provided by the invention has good physical and chemical properties and good constructability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of coatings, and specifically relates to a highly rain-erosion-resistant wind turbine blade leading edge protective coating, a preparation method thereof, and an application thereof. Background Art

[0002] Blades are one of the core components of wind turbines. The raw materials used not only determine the performance of the blades themselves, but also determine the overall performance of the wind turbine. The coating used on the blades is one of the five main materials of the blades. Its main function is to protect the blades from strong light, wind and sand, corrosion, high and low temperatures, etc.

[0003] When the blades are running at high speed, the tip speed can reach more than 75m / s. Raindrops will hit the blade surface like bullets. The leading edge, as the main force-bearing surface, is easily damaged. In order to protect the leading edge of the blade, highly elastic materials should be used to alleviate the impact force. Coatings are one of the most cost-effective protective materials.

[0004] Leading edge protection coating is a kind of coating with high elasticity. Due to its high elasticity (high tensile strength and elongation), excellent rain erosion resistance, aging resistance, adhesion and flexibility, it can release impact stress, provide corrosion resistance and provide better protection for the blade surface.

[0005] In recent years, with the continuous increase in the power of wind turbines, the continuous increase in the design length of blades, and the rapid development of offshore wind power, the performance requirements for related materials have continued to increase. Traditional leading edge protective coatings are gradually unable to provide long-term protection, resulting in a decrease in the operating efficiency of wind turbines. Summary of the invention

[0006] In response to the deficiencies in the prior art, the present application provides a coating, a preparation method thereof, and an application thereof. The coating of the present application is a mixture of two polyaspartic acid ester resins, which not only gives the paint film an ultra-high elongation, but also gives the paint film an ultra-high tensile strength, which can provide more excellent rain erosion resistance. The IPDI-based aliphatic isocyanate prepolymer used in the present application can enable the paint film to maintain an ultra-high elongation and ultra-high tensile strength at low temperatures, and can ensure that the paint film still has excellent rain erosion resistance at low temperatures. The coating of the present application has good physical and chemical properties and good workability. The coating of the present application does not contain heavy metals and is more environmentally friendly, healthy, and safe.

[0007] In one aspect, the present application provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.8-1.1, wherein the composition of the component one is: 15-25 parts of polyaspartic acid resin A, 15-25 parts of polyaspartic acid resin B, 0.5-1.5 parts of dispersant, 1-3 parts of defoamer, 1-4 parts of water absorbent, 0.5-1 parts of leveling agent, 0.2-1 parts of thixotropic agent, 1-3 parts of light absorber, 1-2 parts of light stabilizer, and 30-50 parts of pigment, wherein the total content of the polyaspartic acid resin A and the polyaspartic acid resin B is controlled at 40 parts;

[0008] The composition of the second component is: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

[0009] In an embodiment of the present application, the polyaspartic acid resin A is NH1420 of Covestro, the polyaspartic acid resin B is NH1220 of Covestro, and the dispersant is any one of BYK-161, BYK-163, AFCONA-4046 and AFCONA-4063.

[0010] In an embodiment of the present application, the defoaming agent is any one of AFCONA-2620-85D1, BYK-A525, BYK-1796 and BYK-1799.

[0011] In an embodiment of the present application, the water absorbent is any one of molecular sieves, aldimines, oxazolidines and ketimines.

[0012] In an embodiment of the present application, the leveling agent is any one of BYK-320, BYK-322 and BYK-323.

[0013] In an embodiment of the present application, the thixotropic agent is any one of fumed silica, polyamide wax and organic bentonite.

[0014] In an embodiment of the present application, the light absorber is any one of Tinuvin 1130, Tinuvin 328 and TINUVIN 99-2; the light stabilizer is any one of Tinuvin 292, TINUVIN 123 and Tinuvin 770DF.

[0015] In an embodiment of the present application, the pigment is one of rutile titanium dioxide, carbon black, and light-fast yellow, or a combination thereof.

[0016] In the embodiment of the present application, the component two is E 40480MPA.

[0017] On the other hand, the present application provides a method for preparing the coating as described above, comprising the following steps:

[0018] a. Preparation of component 1:

[0019] (1) adding polyaspartic acid resin A, polyaspartic acid resin B, dispersant, defoamer, water absorbent, thixotropic agent and pigment into a preparation pot according to the weight ratio, and dispersing at a high speed of 800-1000 r / min until there is no obvious powder block to obtain a paint slurry;

[0020] (2) grinding the paint slurry until the fineness is 15-25 μm,

[0021] (3) adding the leveling agent, light absorber and light stabilizer to the ground paint slurry in the weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20-30 minutes to obtain component 1;

[0022] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.8-1.1, and stirred evenly to obtain a coating.

[0023] In another aspect, the present application provides use of the coating as described above or the coating prepared according to the method as described above as a coating for protecting the leading edge of a wind turbine blade.

[0024] The coating of the present application is a mixture of two polyaspartic acid ester resins, which not only gives the paint film an ultra-high elongation, but also an ultra-high tensile strength, which can provide more excellent rain erosion resistance. The IPDI-based aliphatic isocyanate prepolymer used in the present application can make the paint film still maintain an ultra-high elongation and ultra-high tensile strength at low temperatures, and can ensure that the paint film still has excellent rain erosion resistance at low temperatures. The coating of the present application has good physical and chemical properties and good workability. The coating of the present application does not contain heavy metals and is more environmentally friendly, healthy and safe.

[0025] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be realized and obtained by the schemes described in the description. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application will be described in detail below. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.

[0027] The embodiment of the present application provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.8-1.1, wherein the composition of the component one is: 15-25 parts of polyaspartic acid resin A, 15-25 parts of polyaspartic acid resin B, 0.5-1.5 parts of dispersant, 1-3 parts of defoamer, 1-4 parts of water absorbent, 0.5-1 parts of leveling agent, 0.2-1 parts of thixotropic additive, 1-3 parts of light absorber, 1-2 parts of light stabilizer, and 30-50 parts of pigment, wherein the total content of the polyaspartic acid resin A and the polyaspartic acid resin B is controlled at 40 parts;

[0028] The composition of the second component is: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

[0029] In an embodiment of the present application, the polyaspartic acid resin A is NH1420 of Covestro, the polyaspartic acid resin B is NH1220 of Covestro, and the dispersant is any one of BYK-161, BYK-163, AFCONA-4046 and AFCONA-4063.

[0030] In the embodiments of the present application, the defoaming agent is any one of AFCONA-2620-85D1, BYK-A525, BYK-1796 and BYK-1799.

[0031] In an embodiment of the present application, the water absorbent is any one of molecular sieves, aldimines, oxazolidines and ketimines.

[0032] In the embodiments of the present application, the leveling agent is any one of BYK-320, BYK-322 and BYK-323.

[0033] In an embodiment of the present application, the thixotropic agent is any one of fumed silica, polyamide wax and organic bentonite.

[0034] In the embodiments of the present application, the light absorber is any one of Tinuvin 1130, Tinuvin 328 and TINUVIN 99-2; the light stabilizer is any one of Tinuvin 292, TINUVIN 123 and Tinuvin 770DF.

[0035] In an embodiment of the present application, the pigment is one of rutile titanium dioxide, carbon black, and light-fast yellow, or a combination thereof.

[0036] In the embodiments of the present application, the component 2 is E 40480MPA.

[0037] The present application also provides a method for preparing the coating as described above, comprising the following steps:

[0038] a. Preparation of component 1:

[0039] (1) adding polyaspartic acid resin A, polyaspartic acid resin B, dispersant, defoamer, water absorbent, thixotropic agent and pigment into a preparation pot according to the weight ratio, and dispersing at a high speed of 800-1000 r / min until there is no obvious powder block to obtain a paint slurry;

[0040] (2) grinding the paint slurry until the fineness is 15-25 μm,

[0041] (3) adding the leveling agent, light absorber and light stabilizer to the ground paint slurry in the weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20-30 minutes to obtain component 1;

[0042] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.8-1.1, and stirred evenly to obtain a coating.

[0043] The embodiments of the present application also provide the use of the coating as described above or the coating prepared according to the method as described above as a coating for protecting the leading edge of a wind turbine blade.

[0044] The sources of materials used in the examples and comparative examples of this application are as follows:

[0045] Polyaspartic acid resin A is NH1420 from Covestro; polyaspartic acid resin B is NH1220 from Covestro; dispersant is BYK-163; defoamer is BYK-1799; water absorbent is 4A molecular sieve; leveling agent is BYK-320; thixotropic additive is fumed silica; light absorber is 1130; Light stabilizer is 292; Pigments are rutile titanium dioxide, carbon black, and light-fast yellow; Component 2, IPDI-based aliphatic isocyanate prepolymer is from Covestro E40480MPA; HDI-based aliphatic polyisocyanate prepolymer from Covestro N3600.

[0046] Example 1

[0047] The present embodiment provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.85, wherein the component one is composed of: 20 parts of polyaspartic acid ester resin A, 20 parts of polyaspartic acid ester resin B, 1 part of dispersant, 3 parts of defoamer, 4 parts of water absorbent, 0.5 parts of leveling agent, 0.5 parts of thixotropic additive, 2 parts of light absorber, 2 parts of light stabilizer, 46.4 parts of rutile titanium dioxide, 0.2 parts of carbon black, and 0.4 parts of light-fast yellow;

[0048] The composition of the second component is: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

[0049] The coating of this embodiment is prepared by a method comprising the following steps:

[0050] a. Preparation of component 1:

[0051] (1) adding resin, dispersant, defoamer, water absorbent, thixotropic agent and pigment into a preparation pot according to the weight ratio, and dispersing at a high speed of 800-1000 r / min until there is no obvious powder block, thereby obtaining a paint slurry;

[0052] (2) grinding the paint slurry until the fineness is 15-25 μm;

[0053] (3) adding the leveling agent, light absorber and light stabilizer to the ground paint slurry in the weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20 minutes to obtain component 1;

[0054] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.85, and stirred evenly to obtain a coating.

[0055] Embodiment 2:

[0056] The present embodiment provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.85, wherein the component one is composed of: 15 parts of polyaspartic acid ester resin A, 25 parts of polyaspartic acid ester resin B, 1 part of dispersant, 3 parts of defoamer, 4 parts of water absorbent, 0.5 parts of leveling agent, 0.5 parts of thixotropic agent, 2 parts of light absorber, 2 parts of light stabilizer, 46.4 parts of rutile titanium dioxide, 0.2 parts of carbon black, and 0.4 parts of light-fast yellow;

[0057] The second component consists of: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

[0058] The coating of this embodiment is prepared by a method comprising the following steps:

[0059] a. Preparation of component 1:

[0060] (1) adding resin, dispersant, defoamer, water absorbent, thixotropic additive, and pigment rutile titanium dioxide into a preparation pot according to the weight ratio, and dispersing at a high speed of 800-1000 r / min until there is no obvious powder block to obtain a paint slurry;

[0061] (2) grinding the paint slurry until the fineness is 15-25 μm;

[0062] (3) adding the leveling agent, light absorber and light stabilizer to the paint slurry with qualified fineness in the above weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20 minutes to obtain component 1;

[0063] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.85, and stirred evenly to obtain a coating.

[0064] Example 3

[0065] The present embodiment provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.85, wherein the component one is composed of: 25 parts of polyaspartic acid ester resin A, 15 parts of polyaspartic acid ester resin B, 1 part of dispersant, 3 parts of defoamer, 4 parts of water absorbent, 0.5 parts of leveling agent, 0.5 parts of thixotropic agent, 2 parts of light absorber, 2 parts of light stabilizer, 46.4 parts of rutile titanium dioxide, 0.2 parts of carbon black, and 0.4 parts of light-fast yellow;

[0066] The second component consists of: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

[0067] The coating of this embodiment is prepared by a method comprising the following steps:

[0068] a. Preparation of component 1:

[0069] (1) adding resin, dispersant, defoamer, water absorbent, thixotropic additive, and pigment rutile titanium dioxide into a preparation pot according to the weight ratio, and dispersing at a high speed of 800-1000 r / min until there is no obvious powder block to obtain a paint slurry;

[0070] (2) grinding the paint slurry until the fineness is 15-25 μm;

[0071] (3) adding the leveling agent, light absorber and light stabilizer to the paint slurry with qualified fineness in the above weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20 minutes to obtain component 1;

[0072] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.85, and stirred evenly to obtain a coating.

[0073] Comparative Example 1:

[0074] This comparative example provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.85, wherein the component one is composed of: 40 parts of polyaspartic acid ester resin A, 1 part of dispersant, 3 parts of defoamer, 4 parts of water absorbent, 0.5 parts of leveling agent, 0.5 parts of thixotropic additive, 2 parts of light absorber, 2 parts of light stabilizer, 46.4 parts of rutile titanium dioxide, 0.2 parts of carbon black, and 0.4 parts of light-fast yellow;

[0075] The second component consists of: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

[0076] The coating of this comparative example was prepared by a method comprising the following steps:

[0077] a. Preparation of component 1:

[0078] (1) adding resin, dispersant, defoamer, water absorbent, thixotropic agent and rutile titanium dioxide into a preparation pot according to the weight ratio, dispersing at a high speed of 800-1000 r / min until there is no obvious powder block, to obtain a paint slurry;

[0079] (2) grinding the paint slurry until the fineness is 15-25 μm;

[0080] (3) adding the leveling agent, light absorber and light stabilizer to the ground paint slurry in the above weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20 minutes to obtain component one.

[0081] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.85, and stirred evenly to obtain a coating.

[0082] Comparative Example 2:

[0083] This comparative example provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.85, wherein the component one is composed of: 40 parts of polyaspartic acid ester resin B, 1 part of dispersant, 3 parts of defoamer, 4 parts of water absorbent, 0.5 parts of leveling agent, 0.5 parts of thixotropic additive, 2 parts of light absorber, 2 parts of light stabilizer, 46.4 parts of rutile titanium dioxide, 0.2 parts of carbon black, and 0.4 parts of light-fast yellow;

[0084] The second component consists of: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

[0085] The coating of this comparative example was prepared by a method comprising the following steps:

[0086] a. Preparation of component 1:

[0087] (1) Add resin, dispersant, defoamer, water absorbent, thixotropic agent and rutile titanium dioxide into a preparation pot according to the weight ratio, and disperse at a high speed of 800-1000 r / min until there is no obvious powder block to obtain a paint slurry.

[0088] (2) grinding the paint slurry until the fineness is 15-25 μm;

[0089] (3) adding the leveling agent, light absorber and light stabilizer to the ground paint slurry in the above weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20 minutes to obtain component one.

[0090] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.85, and stirred evenly to obtain a coating.

[0091] Comparative Example 3:

[0092] The present embodiment provides a coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.85, wherein the component one is composed of: 20 parts of polyaspartic acid ester resin A, 20 parts of polyaspartic acid ester resin B, 1 part of dispersant, 3 parts of defoamer, 4 parts of water absorbent, 0.5 parts of leveling agent, 0.5 parts of thixotropic additive, 2 parts of light absorber, 2 parts of light stabilizer, 46.4 parts of rutile titanium dioxide, 0.2 parts of carbon black, and 0.4 parts of light-fast yellow;

[0093] The composition of the second component is: 100 parts of HDI-based aliphatic polyisocyanate prepolymer.

[0094] The coating of this embodiment is prepared by a method comprising the following steps:

[0095] a. Preparation of component 1:

[0096] (1) adding resin, dispersant, defoamer, water absorbent, thixotropic agent and pigment into a preparation pot according to the weight ratio, and dispersing at a high speed of 800-1000 r / min until there is no obvious powder block, thereby obtaining a paint slurry;

[0097] (2) grinding the paint slurry until the fineness is 15-25 μm;

[0098] (3) adding the leveling agent, light absorber and light stabilizer to the ground paint slurry in the weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20 minutes to obtain component 1;

[0099] b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.85, and stirred evenly to obtain a coating.

[0100] Performance Testing

[0101] The coatings prepared in Examples 1-3 and Comparative Examples 1-3 were applied to the leading edge of a wind turbine blade, and performance tests such as rain erosion resistance and aging resistance were carried out; the specific test results are shown in Table 1 below.

[0102] Table 1

[0103]

[0104]

[0105] From Table 1, we can see that:

[0106] 1. Two complementary polyurea resins are selected in the coating of the present application, wherein the polyaspartic acid ester resin A is a component with weaker elasticity, having high tear strength and low tear elongation; the polyaspartic acid ester resin B is a component with higher elasticity, having low tear strength and high tear elongation; the two resins are mixed and used, and the complementary properties achieve the optimal performance;

[0107] 2. The compatibility of polyaspartic acid resin A and polyaspartic acid resin B is excellent. The prepared coating has good rain erosion resistance and no breakdown after 20 hours; and no breakdown after 10 hours after artificial accelerated aging UVB for 2000 hours;

[0108] 3. Through the test of comparative example 3, the performance of HDI aliphatic polyisocyanate and IPDI aliphatic polyisocyanate is different: the rain erosion resistance of HDI aliphatic polyisocyanate is significantly reduced.

[0109] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of patent protection of this application shall still be based on the scope defined in the attached claims.

Claims

1. A coating, wherein the raw materials of the coating include component one and component two, wherein the component one and component two are mixed in a ratio of NCO / NH=0.8-1.1, wherein: The composition of the component one is: 15-25 parts of polyaspartic acid resin A, 15-25 parts of polyaspartic acid resin B, 0.5-1.5 parts of dispersant, 1-3 parts of defoamer, 1-4 parts of water absorbent, 0.5-1 parts of leveling agent, 0.2-1 parts of thixotropic additive, 1-3 parts of light absorber, 1-2 parts of light stabilizer, 30-50 parts of pigment, wherein the total content of the polyaspartic acid resin A and the polyaspartic acid resin B is controlled at 40 parts; The composition of the second component is: 100 parts of IPDI-based aliphatic isocyanate prepolymer.

2. The coating according to claim 1, wherein The polyaspartic acid resin A is NH1420 produced by Covestro, the polyaspartic acid resin B is NH1220 produced by Covestro, and the dispersant is any one of BYK-161, BYK-163, AFCONA-4046 and AFCONA-4063.

3. The coating according to claim 1, wherein The defoamer is any one of AFCONA-2620-85D1, BYK-A525, BYK-1796 and BYK-1799.

4. The coating according to claim 1, wherein The water absorbent is any one of molecular sieves, aldimines, oxazolidines and ketimines.

5. The coating according to claim 1, wherein The leveling agent is any one of BYK-320, BYK-322 and BYK-323.

6. The coating according to claim 1, wherein The thixotropic additive is any one of fumed silica, polyamide wax and organic bentonite.

7. The coating according to claim 1, wherein The light absorber is any one of Tinuvin 1130, Tinuvin 328 and TINUVIN 99-2; the light stabilizer is any one of Tinuvin 292, TINUVIN 123 and Tinuvin 770DF.

8. The coating according to claim 1, wherein The pigment is one of rutile titanium dioxide, carbon black and lightfast yellow or a combination thereof.

9. The coating according to any one of claims 1 to 8, wherein The second component is E40480MPA.

10. A method for preparing a coating according to any one of claims 1 to 9, comprising the following steps: a. Preparation of component 1: (1) adding polyaspartic acid resin A, polyaspartic acid resin B, dispersant, defoamer, water absorbent, thixotropic agent and pigment into a preparation pot according to the weight ratio, and dispersing at a high speed of 800-1000 r / min until there is no obvious powder block to obtain a paint slurry; (2) grinding the paint slurry until the fineness is 15-25 μm, (3) adding the leveling agent, light absorber and light stabilizer to the ground paint slurry in the weight ratio while stirring, and dispersing at a high speed of 1000-1200 r / min for 20-30 minutes to obtain component 1; b. Component 1 and component 2 are mixed in a ratio of NCO / NH=0.8-1.1, and stirred evenly to obtain a coating.

11. Use of the coating according to any one of claims 1 to 9 or the coating prepared by the method according to claim 10 as a coating for protecting the leading edge of a wind turbine blade.

Citation Information

Patent Citations

  • Thick paste quick-drying type weather-resistant and wear-resistant coating for wind turbine blades and preparation method thereof

    CN102391771A

  • High-weather-resistance high-solid-content polyaspartic acid ester finish paint and preparation method thereof

    CN115926595A

  • Thin coating type high-corrosion-resistance high-solid-content polyaspartic acid ester primer and preparation method thereof

    CN116376410A