Preparation method of carbon nanotube MXene polytetrafluoroethylene wax polyurea resin composite coating

By growing carbon nanotubes on MXene and mixing them with functionalized polytetrafluoro wax and polyurea resin, the carbon nanotube/MXene/polytetrafluoro wax/polyurea resin composite coating is solved, and the brittleness and wear resistance of polyurea resin are formed. The problem of poor performance has achieved the improvement of high mechanical strength, lubricating performance and self-repair performance, and the preparation process is environmentally friendly and low-cost.

CN118931342AActive Publication Date: 2024-11-12JIANGSU TIANWO HEAVY IND TECH CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411170913.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The pure polyurea resin has high brittleness and poor wear resistance after curing, which limits its application range. The prior art requires unnecessary removal steps and is costly when improving friction and wear performance.

Method used

Using the composite coating preparation method of carbon nanotube MXene and functionalized polytetrafluoro wax and polyurea resin, carbon nanotubes are grown on MXene and formed with high mechanical strength and self-strength through simple chemical vapor deposition and stirring process. Composite coatings for lubricating and self-healing properties.

Benefits of technology

It obtains a composite coating with high mechanical strength, excellent lubricating properties, high wear resistance and fast self-repair performance, and the preparation process is environmentally friendly and pollution-free, and is low-cost, suitable for multifunctional material applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931342A_ABST
    Figure CN118931342A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating, which comprises the following steps: preparing a solution according to the mass ratio of ferrocene to ethylenediamine to ethanol of 0.5 g: 10mL: 40-60mL, dropwise adding 0.1-0.3 g of MXene nanosheet in a nitrogen atmosphere at 800-1000 DEG C to grow a carbon nanotube in situ so as to obtain CNTs / MXene; stirring according to the ratio of the mass of polytetrafluoroethylene wax to the mass of dopamine hydrochloride to the volume of a Tris buffer solution of 1g: 1g: (50-75) mL, and then centrifuging, separating and cleaning to obtain PFW-coated PDA; mixing the CNTs / MXene, the PFW-coated PDA and the polyurea resin slurry according to the mass ratio of 1: 10: (50-200), and stirring to obtain mixed slurry; and coating on a steel sheet, and drying to obtain the composite coating. According to the method, the composite coating with good mechanical strength, excellent lubricating property and high wear resistance can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and specifically relates to a method for preparing a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating. Background Art

[0002] Friction and wear are everywhere in life. Friction and wear have caused a large number of device damage, failures, shortened lifespans, and increased use of fuel resources, leading to serious waste of resources and energy. Friction and wear always go hand in hand. Wear not only brings great energy loss, but also causes damage to parts. It makes the machinery fail and unable to work normally, wastes a lot of manpower and material resources, and even endangers life and health. Wear also produces a large amount of "waste", which in turn brings great pressure to the environment. Polymer-based wear-resistant composite materials not only have excellent properties such as friction reduction and wear resistance, but also have excellent properties such as high specific strength and simple processing. Choosing suitable resin-based wear-resistant composite materials can not only solve many technical problems that are difficult to overcome using metal materials, improve the service life and safety of machinery and equipment, reduce the occurrence of safety accidents, but also improve the technical indicators of the machine structure, thereby saving a large amount of precious metal materials, reducing the total weight of machinery and equipment, and reducing the overall manufacturing cost.

[0003] The commonly used resin bases for polymer solid lubricating coatings are polyurea resins, phenolic resins, silicone resins, polyurethanes, etc. Polyurea resins have good adhesion, corrosion resistance and chemical stability, as well as low curing shrinkage and easy processing and molding. This has created an absolute leading position for polyurea resin-based composite coatings in real life use, and it has also become a key material for research by a large number of scientific researchers.

[0004] Polyurea resin has the above-mentioned excellent physical and chemical properties, which means it is destined to be able to play its own characteristics in various fields. Therefore, the application of polyurea resin and its composite materials covers various fields. However, pure polyurea resin is highly brittle and has poor wear resistance after curing, which seriously limits the application of polyurea resin. In order to enable it to have a broader development space, people have been committed to enhancing and modifying polyurea resin. Physical methods are the most effective and most commonly used methods to improve the tribological properties of polyurea coatings. Physical methods refer to filling additives in the polyurea resin coating matrix to improve the friction and wear properties of the coating. For example, adding solid lubricants to the coating can effectively improve the hardness, stiffness and load-bearing capacity of the coating, thereby improving the creep resistance and compression properties of the composite material, and then improving the friction properties of the coating. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for preparing a carbon nanotube MXene polytetrafluorowax polyurea resin composite coating. The method has a simple preparation process, low manufacturing cost, and an environmentally friendly and pollution-free manufacturing process, and can obtain a carbon nanotube / MXene / polytetrafluorowax / polyurea composite coating with good mechanical strength, excellent lubrication performance, high wear resistance and rapid self-repairing performance.

[0006] The present invention provides a method for preparing a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating, comprising the following steps:

[0007] Step 1: Prepare a solution for growing carbon nanotubes according to the mass of ferrocene, the volume of ethylenediamine, and the volume ratio of ethanol to be 0.5 g ﹕ 10 mL ﹕ 40-60 mL, and slowly drop the prepared solution on 0.1-0.3 g MXene nanosheets in a nitrogen atmosphere at 800-1000° C. to in-situ grow carbon nanotubes to obtain CNTs / MXene;

[0008] Step 2: Add polytetrafluoro wax and dopamine hydrochloride into Tris buffer according to the ratio of the mass of polytetrafluoro wax, the mass of dopamine hydrochloride and the volume ratio of Tris buffer of 1g:1g:50-75mL and stir continuously. After the end, centrifuge, separate and wash with distilled water for 3-5 times to obtain polydopamine functionalized PFW@PDA;

[0009] Step 3: Mix the CNTs / MXene, PFW@PDA and polyurea resin slurry in a mass ratio of 1:10:50-200, and stir at a speed of 900 rpm for 20-24 hours to obtain a mixed slurry;

[0010] Step 4: Apply the mixed slurry obtained in step 3 on a steel sheet and dry it at room temperature for 24 to 48 hours to obtain a self-lubricating CNT / MXene / PFW@PDA / polyurea resin composite coating.

[0011] As a preferred embodiment, in the Tris buffer in step 2, a uniform solution of 2.4465 g Tris and 0.4221 g concentrated hydrochloric acid is added to 300 mL distilled water; the stirring time is 20 to 24 hours; and the centrifugal speed is 8000 rpm.

[0012] As a preference, in step three, the mass ratio of the polyurea resin slurry to its curing agent is 1:2-3.

[0013] As a preferred embodiment, in step 4, the steel sheet is pretreated before coating, and the pretreatment method is as follows:

[0014] The steel sheet was cleaned 3 to 5 times using a mixed solution of ethanol and acetone in a mass ratio of 1:1.

[0015] Compared with the prior art, the present invention has the following technical effects:

[0016] 1. The preparation method of the present invention is very simple and does not require any extra impurity removal steps. The solvent used in the entire preparation process is green, environmentally friendly and pollution-free. It only requires simply etching MXene, growing carbon nanotubes on MXene by chemical vapor deposition, mixing the functionalized polytetrafluoroethylene wax and carbon nanotube / MXene powder with polyurea resin slurry, stirring them fully, and then coating them on a prefabricated steel sheet, and then curing them at room temperature to obtain a carbon nanotube / MXene / polytetrafluoroethylene wax / polyurea resin composite coating;

[0017] 2. The composite coating obtained by the present invention shows high mechanical strength, excellent self-lubricating properties, high wear resistance, and excellent self-repairing properties. The composite coating can still remain intact under the impact of an iron ball, and the composite coating composite film still maintains structural stability under high temperatures. It is characterized by the nano-scale entanglement and hydrogen bonds between graphene, Mxene and cellulose micro-nano fibrils. Since the entangled micro / nano cellulose itself acts as a reinforcing phase, it interacts with the micro / nano cellulose through hydrogen bonds and van der Waals forces to form a strong hybrid interwoven structure. The composite PVA has a denser structure, giving the multifunctional material excellent mechanical properties; due to the dense structure of the multifunctional material, it is difficult for water molecules to invade the interior of the material, so it has good stability in water; after the thermal conductivity test of the wood cellulose friction material, it was found that it has excellent thermal conductivity and photothermal conversion performance, and the material has low thickness, high mechanical strength and excellent flexibility;

[0018] 3. The raw material used in the present invention is corn stalk powder, an agricultural waste material. As a typical green natural biomass material, it has the advantages of wide sources, large reserves, green environmental protection, and low price;

[0019] 4. The synthesis process of the present invention is simple and does not require overly complicated synthesis steps. It shows great potential in thermal management applications such as flexible heat sinks, wearable technology, personal thermal management, skin electronics and energy storage devices;

[0020] 5. The material prepared by the present invention has extremely high sustainability. Not only can it be recycled using laboratory methods, but also because its material composition uses cellulose and degradable PVA as the main skeleton, it can be degraded by microorganisms in the natural environment and has a lower impact on the environment.

[0021] 6. The raw materials of the present invention are widely available, the preparation process is simple, the cost is low, and it is environmentally friendly and pollution-free. The prepared carbon nanotube / MXene / polytetrafluoro wax / polyurea composite coating has good mechanical strength, excellent lubrication performance, high wear resistance and rapid self-repairing performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a SEM microstructure diagram of the MXene prepared by the present invention;

[0023] Figure 2 is a SEM microstructure image of CNTs / MXene prepared by the present invention;

[0024] Figure 3 This is the SEM microstructure of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared by the present invention

[0025] Figure 4 It is a macroscopic photograph of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared by the present invention;

[0026] Figure 5 It is a friction coefficient diagram of the dry friction environment of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared by the present invention;

[0027] Figure 6 It is a friction coefficient diagram of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared by the present invention in an oil friction environment;

[0028] Figure 7 It is a long-term friction coefficient diagram of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared by the present invention;

[0029] Figure 8 This is a wear scar morphology diagram of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared in the present invention. DETAILED DESCRIPTION

[0030] The present invention provides a method for preparing a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating, comprising the following steps:

[0031] Step 1: Prepare a solution for growing carbon nanotubes according to the mass of ferrocene, the volume of ethylenediamine, and the volume ratio of ethanol to be 0.5 g ﹕ 10 mL ﹕ 40-60 mL, and slowly drop the prepared solution on 0.1-0.3 g MXene nanosheets in a nitrogen atmosphere at 800-1000° C. to in-situ grow carbon nanotubes to obtain CNTs / MXene (carbon nanotube / MXene powder);

[0032] Step 2: Add polytetrafluoro wax and dopamine hydrochloride into Tris buffer according to the ratio of the mass of polytetrafluoro wax, the mass of dopamine hydrochloride and the volume ratio of Tris buffer of 1g:1g:50-75mL and stir continuously, and then centrifuge, separate and wash with distilled water for 3-5 times to obtain polydopamine functionalized PFW@PDA (polytetrafluoro wax);

[0033] Step 3: Mix the CNTs / MXene, PFW@PDA and polyurea resin slurry in a mass ratio of 1:10:50-200, and stir at a speed of 900 rpm for 20-24 hours to obtain a mixed slurry;

[0034] Step 4: Apply the mixed slurry obtained in step 3 on a steel sheet and dry it at room temperature for 24 to 48 hours to obtain a self-lubricating CNT / MXene / PFW@PDA / polyurea resin composite coating.

[0035] As a preferred embodiment, in the Tris buffer in step 2, a uniform solution of 2.4465 g Tris and 0.4221 g concentrated hydrochloric acid is added to 300 mL distilled water; the stirring time is 20 to 24 hours; and the centrifugal speed is 8000 rpm.

[0036] As a preference, in step three, the mass ratio of the polyurea resin slurry to its curing agent is 1:2-3.

[0037] As a preferred embodiment, in step 4, the steel sheet is pretreated before coating, and the pretreatment method is as follows:

[0038] The steel sheet was cleaned 3 to 5 times using a mixed solution of ethanol and acetone in a mass ratio of 1:1.

[0039] Compared with the prior art, the present invention has the following technical effects:

[0040] 1. The preparation method of the present invention is very simple and does not require any extra impurity removal steps. The solvent used in the entire preparation process is green, environmentally friendly and pollution-free. It only requires simply etching MXene, growing carbon nanotubes on MXene by chemical vapor deposition, mixing the functionalized polytetrafluoroethylene wax and carbon nanotube / MXene powder with polyurea resin slurry, stirring them fully, and then coating them on a prefabricated steel sheet, and then curing them at room temperature to obtain a carbon nanotube / MXene / polytetrafluoroethylene wax / polyurea resin composite coating;

[0041] 2. The composite coating obtained by the present invention shows high mechanical strength, excellent self-lubricating properties, high wear resistance, and excellent self-repairing properties. The composite coating can still remain intact under the impact of an iron ball, and the composite coating composite film still maintains structural stability under high temperatures. It is characterized by the nano-scale entanglement and hydrogen bonds between graphene, Mxene and cellulose micro-nano fibrils. Since the entangled micro / nano cellulose itself acts as a reinforcing phase, it interacts with the micro / nano cellulose through hydrogen bonds and van der Waals forces to form a strong hybrid interwoven structure. The composite PVA has a denser structure, giving the multifunctional material excellent mechanical properties; due to the dense structure of the multifunctional material, it is difficult for water molecules to invade the interior of the material, so it has good stability in water; after the thermal conductivity test of the wood cellulose friction material, it was found that it has excellent thermal conductivity and photothermal conversion performance, and the material has low thickness, high mechanical strength and excellent flexibility;

[0042] 3. The raw material used in the present invention is corn stalk powder, an agricultural waste material. As a typical green natural biomass material, it has the advantages of wide sources, large reserves, green environmental protection, and low price;

[0043] 4. The synthesis process of the present invention is simple and does not require overly complicated synthesis steps. It shows great potential in thermal management applications such as flexible heat sinks, wearable technology, personal thermal management, skin electronics and energy storage devices;

[0044] 5. The material prepared by the present invention has extremely high sustainability. Not only can it be recycled using laboratory methods, but also because its material composition uses cellulose and degradable PVA as the main skeleton, it can be degraded by microorganisms in the natural environment and has a lower impact on the environment.

[0045] 6. The raw materials of the present invention are widely available, the preparation process is simple, the cost is low, and it is environmentally friendly and pollution-free. The prepared carbon nanotube / MXene / polytetrafluoro wax / polyurea composite coating has good mechanical strength, excellent lubrication performance, high wear resistance and rapid self-repairing performance.

[0046] The present invention will be further described below in conjunction with specific embodiments:

[0047] Embodiment 1:

[0048] A method for preparing a carbon nanotube / MXene / polytetrafluoroethylene wax / polyurea resin composite coating comprises the following steps:

[0049] Step 1: The mass of ferrocene, the volume of ethylenediamine, and the volume ratio of ethanol are 0.5g﹕10mL﹕40mL to prepare a solution for growing carbon nanotubes, and the prepared solution is slowly dripped onto 0.1g MXene nanosheets in a nitrogen atmosphere at 900°C to in-situ grow carbon nanotubes to obtain carbon nanotube / MXene powder (CNTs / MXene);

[0050] Step 2: Weigh 1 g of polytetrafluoro wax and 1 g of dopamine hydrochloride and mix with 50 mL of Tris buffer and stir continuously. After the mixture is centrifuged, separated, and washed with distilled water for 4 times, polydopamine functionalized polytetrafluoro wax (PFW@PDA) is obtained.

[0051] Step 3: Weigh 0.02 g of CNTs / MXene and 0.2 g of PFW@PDA and mix with 1 g of polyurea resin slurry and stir (900 rpm) for 20 hours;

[0052] Step 4: The mixed slurry obtained in step 3 is evenly coated on the steel sheet, and dried at room temperature for 36 hours to obtain a carbon nanotube / MXene / polytetrafluoro wax / polyurea resin composite coating.

[0053] Embodiment 2:

[0054] A method for preparing a carbon nanotube / MXene / polytetrafluoroethylene wax / polyurea resin composite coating comprises the following steps:

[0055] Step 1: The mass of ferrocene, the volume of ethylenediamine, and the volume ratio of ethanol are 0.5 g ﹕ 10 mL ﹕ 50 mL to prepare a solution for growing carbon nanotubes, and the prepared solution is slowly dripped on 0.15 g of MXene nanosheets under a nitrogen atmosphere at 800 ° C to in-situ grow carbon nanotubes to obtain carbon nanotube / MXene powder (CNTs / MXene);

[0056] Step 2: Weigh 1 g of polytetrafluoro wax and 1 g of dopamine hydrochloride and mix with 60 mL of Tris buffer and stir continuously. After the mixture is centrifuged, separated, and washed with distilled water for 5 times, polydopamine functionalized polytetrafluoro wax (PFW@PDA) is obtained.

[0057] Step 3: Weigh 0.01 g of CNTs / MXene and 0.1 g of PFW@PDA and mix with 1 g of polyurea resin slurry and stir (900 rpm) for 24 hours;

[0058] Step 4: The mixed slurry obtained in step 3 is evenly coated on the steel sheet, and dried at room temperature for 48 hours to obtain a carbon nanotube / MXene / polytetrafluoro wax / polyurea resin composite coating.

[0059] Embodiment 3:

[0060] A method for preparing a carbon nanotube / MXene / polytetrafluoroethylene wax / polyurea resin composite coating comprises the following steps:

[0061] Step 1: The mass of ferrocene, the volume of ethylenediamine, and the volume ratio of ethanol are 0.5g﹕10mL﹕50mL to prepare a solution for growing carbon nanotubes, and the prepared solution is slowly dripped on 0.3g MXene nanosheets under a nitrogen atmosphere at 1000°C to in-situ grow carbon nanotubes to obtain carbon nanotube / MXene powder (CNTs / MXene);

[0062] Step 2: Weigh 1 g of polytetrafluoro wax and 1 g of dopamine hydrochloride and mix with 65 mL of Tris buffer and stir continuously. After the mixture is centrifuged, separated, and washed with distilled water for 3 times, polydopamine functionalized polytetrafluoro wax (PFW@PDA) is obtained.

[0063] Step 3: Weigh 0.02 g of CNTs / MXene and 0.2 g of PFW@PDA and mix with 2 g of polyurea resin slurry and stir (900 rpm) for 22 hours;

[0064] Step 4: The mixed slurry obtained in step 3 is evenly coated on a steel sheet, and dried at room temperature for 40 hours to obtain a carbon nanotube / MXene / polytetrafluoro wax / polyurea resin composite coating.

[0065] Embodiment 4:

[0066] A method for preparing a carbon nanotube / MXene / polytetrafluoroethylene wax / polyurea resin composite coating comprises the following steps:

[0067] Step 1: The mass of ferrocene, the volume of ethylenediamine, and the volume ratio of ethanol are 0.5g﹕10mL﹕50mL to prepare a solution for growing carbon nanotubes, and the prepared solution is slowly dripped on 0.2g MXene nanosheets under a nitrogen atmosphere at 900°C to in-situ grow carbon nanotubes to obtain carbon nanotube / MXene powder (CNTs / MXene);

[0068] Step 2: Weigh 1 g of polytetrafluoro wax and 1 g of dopamine hydrochloride and mix with 75 mL of Tris buffer and stir continuously. After the mixture is centrifuged, separated, and washed with distilled water for 5 times, polydopamine functionalized polytetrafluoro wax (PFW@PDA) is obtained.

[0069] Step 3: Weigh 0.015 g of CNTs / MXene and 0.15 g of PFW@PDA and mix with 1 g of polyurea resin slurry and stir (900 rpm) for 24 hours;

[0070] Step 4: The mixed slurry obtained in step 3 is evenly coated on the steel sheet, and dried at room temperature for 48 hours to obtain a carbon nanotube / MXene / polytetrafluoro wax / polyurea resin composite coating.

[0071] like Figure 1 As shown, it is a SEM image of the MXene prepared in Example 1, and the "accordion"-shaped MXene can be clearly observed, which proves that the etching of MXene is successful.

[0072] like Figure 2 As shown, it is a SEM image of CNTs / MXene prepared in Example 1. It can be found that CNTs grow in situ between MXene layers to form a material with a CNTs / MXene structure, which fully proves the successful preparation of CNTs / MXene.

[0073] like Figure 3 As shown, it is a SEM image of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared in Example 4. It can be found that the surface is uneven, which is caused by the mixture of PFW@PDA and CNTs / MXene, which also confirms that the composite coating is successfully prepared.

[0074] like Figure 4 As shown, it is a macroscopic photograph of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared in Example 4. The coating surface has no bubbles and has excellent mechanical strength.

[0075] like Figure 5 As shown, it is a friction coefficient curve of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared in Example 4 in a dry friction environment. Compared with the polyurea resin coating, its friction coefficient is reduced by 79.5%.

[0076] like Figure 6 As shown, it is a friction coefficient curve of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared in Example 4 in an oil friction environment. Compared with the polyurea resin coating, its friction coefficient is reduced by 96.7%.

[0077] like Figure 7 As shown, it is a friction coefficient curve of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared in Example 4 under a long-term friction environment. The composite coating can maintain a stable friction coefficient for a long time.

[0078] like Figure 8As shown, it is a wear scar morphology of the CNT / MXene / PFW@PDA / polyurea resin composite coating prepared in Example 4 under a long-term friction environment. The wear scar morphology has no obvious damage, proving that the composite coating can be used for a long time.

Claims

1. A method for preparing a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating, characterized in that: The steps include: Step 1: Prepare a solution for growing carbon nanotubes according to the mass of ferrocene, the volume of ethylenediamine, and the volume ratio of ethanol to be 0.5 g ﹕ 10 mL ﹕ 40-60 mL, and slowly drop the prepared solution on 0.1-0.3 g MXene nanosheets in a nitrogen atmosphere at 800-1000° C. to in-situ grow carbon nanotubes to obtain CNTs / MXene; Step 2: Add polytetrafluoro wax and dopamine hydrochloride into Tris buffer according to the ratio of the mass of polytetrafluoro wax, the mass of dopamine hydrochloride and the volume ratio of Tris buffer of 1g:1g:50-75mL and stir continuously. After the end, centrifuge, separate and wash with distilled water for 3-5 times to obtain polydopamine functionalized PFW@PDA; Step 3: Mix the CNTs / MXene, PFW@PDA and polyurea resin slurry in a mass ratio of 1:10:50-200, and stir at a speed of 900 rpm for 20-24 hours to obtain a mixed slurry; Step 4: Apply the mixed slurry obtained in step 3 on a steel sheet and dry it at room temperature for 24 to 48 hours to obtain a self-lubricating CNT / MXene / PFW@PDA / polyurea resin composite coating.

2. The method for preparing a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating according to claim 1, characterized in that: In the Tris buffer solution prepared in step 2, add a uniform solution of 2.4465 g Tris and 0.4221 g concentrated hydrochloric acid to 300 mL distilled water; stir for 20 to 24 hours; and centrifuge at 8000 rpm.

3. The method for preparing a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating according to claim 1 or 2, characterized in that: In step three, the mass ratio of the polyurea resin slurry to its curing agent is 1:2-3.

4. The method for preparing a carbon nanotube MXene polytetrafluoro wax polyurea resin composite coating according to claim 3, characterized in that: In step 4, the steel sheet is pretreated before coating, and the pretreatment method is as follows: The steel sheet was cleaned 3 to 5 times using a mixed solution of ethanol and acetone in a mass ratio of 1:1.

Citation Information

Patent Citations

  • Titanium carbide in-situ growth CNTs three-dimensional composite with polydopamine serving as transition layer and preparation method thereof

    CN106698430A

  • Preparation method of polyurea composite coating with wear-resistant and self-repairing functions

    CN113337192A

  • MXene-coated oriented carbon nanotube composite film as well as preparation method and application thereof

    CN114749353A

  • Preparation method of MXene / CNT composite sponge reinforced resin-based composite material

    CN115073886A

  • Micro-nano cellulose limited MXene / PFW-coated PDA oil-based lubricant and preparation method thereof

    CN116286144A