Coating with formaldehyde decomposition function and preparation method thereof
By using aloe juice, bioenzymes and photocatalysts in the paint, combined with specific formulas and processes, the shortcomings of existing paints in formaldehyde removal and antibacterial are solved, and the uniform formaldehyde decomposition and antibacterial performance of the paint is achieved, reducing the environment pollute.
Patent Information
- Application Number
- CN202411115008.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
Existing paints have poor effects in removing formaldehyde and antibacterial, and it is difficult to solve both problems at the same time, resulting in uneven formaldehyde decomposition and poorer effects after long-term use.
Aloe vera juice is used to improve the antibacterial and soil resistance of paint, biological enzymes improve degradability, photocatalysts enhance antibacterial and mildew resistance, and combined with ultra-hydrophilic self-cleaning function, paints with formaldehyde decomposition functions are prepared using specific formulas and processes.
It realizes uniform formaldehyde decomposition of the paint, improves antibacterial and mildew resistance, enhances the degradability and self-cleaning function of the paint, and reduces the pollution of the waste to the environment.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and specifically refers to a coating with formaldehyde decomposition function and a preparation method thereof. Background Art
[0002] The sources of formaldehyde in indoor environments are mainly furniture and fabrics, wood product fillers, construction sources, detergents, cosmetics and personal products, among which artificial boards are the main ones. Formaldehyde is irritating to the skin and mucous membranes. Inhalation of formaldehyde can cause symptoms such as dizziness, headache, fatigue, nausea, and in severe cases, it can also lead to infertility, fetal malformation, and cancer.
[0003] In recent years, in response to the pollution problem of volatile harmful pollutants such as formaldehyde and benzene generated by indoor decoration, major manufacturers have launched environmentally friendly coatings. However, existing coatings are prone to problems such as uneven dispersion of formaldehyde decomposers and poor formaldehyde removal effects after long-term use. Therefore, coatings in the prior art often find it difficult to simultaneously solve the formaldehyde removal and antibacterial problems. Therefore, a new type of coating with formaldehyde decomposition function and a preparation method thereof are urgently needed to solve the above problems. Summary of the invention
[0004] In order to solve the above-mentioned existing problems, the present invention provides a coating with formaldehyde decomposition function and a preparation method thereof, which improves the antibacterial and anti-fouling properties of paint by aloe vera juice; improves the degradability of paint by biological enzymes, which helps to reduce the pollution of paint waste to the environment; and improves the antibacterial and anti-mildew properties of paint by photocatalysts, and the super-hydrophilic self-cleaning function.
[0005] The technical scheme adopted by the present invention is as follows: The coating with formaldehyde decomposition function of the present invention includes the following raw materials: water, aloe juice, defoaming agent, dispersant, multifunctional additive, titanium dioxide slurry, biological enzyme, photocatalyst, pearl powder, film-forming agent, colorful flakes, fluff powder, activated carbon, thickener, sodium secondary alkyl sulfonate, propylene glycol, and associative thickener.
[0006] The mass parts of each component are: 100 parts of water, 420 parts of aloe juice, 1 part of defoaming agent, 2 parts of dispersant, 2 parts of multifunctional additive, 60 parts of titanium dioxide, 15 parts of biological enzyme, 10 parts of photocatalyst, 170 parts of pearl powder, 25 parts of film-forming agent, 4 parts of colorful flakes, 150 parts of fluff powder, 1 part of activated carbon, 5 parts of thickener, 5 parts of sodium secondary alkyl sulfonate, 10 parts of propylene glycol, and 10 parts of associative thickener.
[0007] Preferably, the dispersant is dispersant 5040, the multifunctional auxiliary agent is AMP-95 multifunctional auxiliary agent, the thickener is TT935 thickener, the secondary alkyl sulfonate is sodium secondary alkyl sulfonate SAS60, and the associative thickener is associative thickener 8w.
[0008] The method for preparing a coating having a formaldehyde decomposition function comprises the following steps:
[0009] S1, put 400 parts of aloe juice, 1 part of defoamer, 2 parts of dispersant, 2 parts of multifunctional additives, 50 parts of water, and 5 parts of sodium secondary alkyl sulfonate into a reaction kettle in sequence, and stir at high speed for 20 minutes;
[0010] S2, add 60 parts of titanium dioxide paste, 20 parts of aloe juice, 15 parts of biological enzyme, 10 parts of photocatalyst, 170 parts of pearl powder, and 25 parts of film-forming agent to the reactor in sequence, and stir at medium speed for 20 minutes;
[0011] S3, add 10 parts of propylene glycol, 3 parts of associative thickener, 4 parts of seven-color flakes, 5 parts of thickener, 50 parts of water, and 150 parts of fluff powder into the reactor, and stir at low speed for 20 minutes;
[0012] S4. Add 1 part of activated carbon into the reactor and let it stand for 60 minutes before filling.
[0013] The beneficial effects achieved by the present invention using the above structure are as follows: the antibacterial and anti-fouling properties of the paint are improved by aloe vera juice; the degradability of the paint is improved by biological enzymes, which helps to reduce the pollution of the environment by paint waste; the antibacterial and anti-mildew properties of the paint, the super-hydrophilic self-cleaning function and the formaldehyde decomposition function are improved by photocatalysts. DETAILED DESCRIPTION
[0014] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0015] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0016] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0017] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0018] Example 1
[0019] The coating with formaldehyde decomposition function includes the following raw materials: water, aloe juice, defoamer, dispersant, multifunctional additive, titanium dioxide slurry, biological enzyme, photocatalyst, pearl powder, film-forming agent, colorful flakes, fluff powder, activated carbon, thickener, sodium secondary alkyl sulfonate, propylene glycol, and associative thickener.
[0020] The method for preparing a coating having a formaldehyde decomposition function comprises the following steps:
[0021] S1, put 400 parts of aloe juice, 1 part of defoamer, 2 parts of dispersant, 2 parts of multifunctional additives, 50 parts of water, and 5 parts of sodium secondary alkyl sulfonate into a reaction kettle in sequence, and stir at high speed for 20 minutes;
[0022] S2, add 60 parts of titanium dioxide paste, 20 parts of aloe juice, 15 parts of biological enzyme, 10 parts of photocatalyst, 170 parts of pearl powder, and 25 parts of film-forming agent to the reactor in sequence, and stir at medium speed for 20 minutes;
[0023] S3, add 10 parts of propylene glycol, 3 parts of associative thickener, 4 parts of seven-color flakes, 5 parts of thickener, 50 parts of water, and 150 parts of fluff powder into the reactor, and stir at low speed for 20 minutes;
[0024] S4. Add 1 part of activated carbon into the reactor and let it stand for 60 minutes before filling.
[0025] The embodiments described above are preferred embodiments of the present invention, rather than all embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A coating having a formaldehyde decomposition function, characterized in that: Including the following ingredients: Water, aloe vera juice, defoamer, dispersant, multifunctional additive, titanium dioxide, biological enzyme, photocatalyst, pearl powder, film-forming agent, colorful flakes, fluff powder, activated carbon, thickener, sodium secondary alkyl sulfonate, propylene glycol, associative thickener.
2. The coating with formaldehyde decomposition function according to claim 1, characterized in that: The mass parts of each component are: 100 parts of water, 420 parts of aloe juice, 1 part of defoaming agent, 2 parts of dispersant, 2 parts of multifunctional additive, 60 parts of titanium dioxide, 15 parts of biological enzyme, 10 parts of photocatalyst, 170 parts of pearl powder, 25 parts of film-forming agent, 4 parts of colorful flakes, 150 parts of fluff powder, 1 part of activated carbon, 5 parts of thickener, 5 parts of sodium secondary alkyl sulfonate, 10 parts of propylene glycol, and 10 parts of associative thickener.
3. The coating with formaldehyde decomposition function according to claim 1, characterized in that: The dispersant is dispersant 5040, the multifunctional auxiliary agent is AMP-95 multifunctional auxiliary agent, the thickener is TT935 thickener, the secondary alkyl sulfonate is sodium secondary alkyl sulfonate SAS60, and the associative thickener is associative thickener 8w.
4. The method for preparing a coating having formaldehyde decomposition function according to claim 1, characterized in that: The following steps are involved: S1, put 400 parts of aloe juice, 1 part of defoamer, 2 parts of dispersant, 2 parts of multifunctional additives, 50 parts of water, and 5 parts of sodium secondary alkyl sulfonate into a reaction kettle in sequence, and stir at high speed for 20 minutes; S2, add 60 parts of titanium dioxide paste, 20 parts of aloe juice, 15 parts of biological enzyme, 10 parts of photocatalyst, 170 parts of pearl powder, and 25 parts of film-forming agent to the reactor in sequence, and stir at medium speed for 20 minutes; S3, add 10 parts of propylene glycol, 3 parts of associative thickener, 4 parts of seven-color flakes, 5 parts of thickener, 50 parts of water, and 150 parts of fluff powder into the reactor, and stir at low speed for 20 minutes; S4. Add 1 part of activated carbon into the reactor and let it stand for 60 minutes before filling.