Buffering silica gel pressure-sensitive adhesive tape with tensile viscosity loss and preparation method of buffering silica gel pressure-sensitive adhesive tape

By using spherical low-molecular methyl MQ silicone resin, end-hydroxylinear silicone oil, high molecular weight silicone rubber and vinyl methyl MQ silicone resin in pressure sensitive tape to form a three-dimensional spatial structure, the existing pressure sensitive tape is solved. The problems of brittleness and loss of stickiness after aging achieve high rebound and buffering performance pressure-sensitive tape, reducing the loss of stickiness caused by vibration drop, and maintaining good performance at high temperatures.

CN118931415AInactive Publication Date: 2024-11-12SHENZHEN KANGLIBANG TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411051673.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing stretched and detachable pressure-sensitive tapes are prone to become brittle and hard after aging, and the solvent volatilizes during the colloid curing process and is prone to bubbles, so it is not possible to have buffering capabilities at the same time, resulting in reduced bonding strength and detachable phenomena.

Method used

The three-dimensional spatial structure is formed by spherical low-molecular methyl MQ silicone resin, end-hydroxyl linear silicone oil, high-molecular weight silicone rubber and vinyl methyl MQ silicone resin. It is made by microsphere foaming agent and small spherical low-molecular methyl MQ silicone. The link reaction of the resin achieves the tensile loss effect of viscosity from existence to none, and introduces methylphenyl resin to prevent oxidation and decomposition, enhancing the rebound and buffering performance of the pressure-sensitive adhesive.

Benefits of technology

It realizes that the pressure-sensitive tape effectively controls the loss of stick during the stretching process, maintains high bonding strength and rebound performance, reduces the loss of sticking caused by vibration drop, and maintains good strength after long-term aging of high temperature and Adhesive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004975103210000081
    Figure BDA0004975103210000081
  • Figure BDA0004975103210000091
    Figure BDA0004975103210000091
Patent Text Reader

Abstract

The invention relates to the technical field of gluing, and particularly discloses a buffer silica gel pressure-sensitive adhesive tape with tensile viscosity loss and a preparation method of the buffer silica gel pressure-sensitive adhesive tape. The invention relates to a buffer silica gel pressure-sensitive adhesive tape with tensile viscosity loss, which is prepared from the following raw materials in parts by weight: 10 to 25 parts of spherical low-molecular-weight methyl MQ silicon resin, 2 to 7 parts of hydroxyl-terminated linear silicone oil, 0.01 to 0.03 part of condensation catalyst, 20 to 35 parts of high-molecular-weight silicone rubber, 40 to 60 parts of vinyl methyl MQ silicon resin, 1 to 5 parts of methyl phenyl resin, 0.8 to 3 parts of hydrogen-containing silicone oil, 0.1 to 2 parts of microsphere foaming agent and 0.01 to 0.03 part of inhibitor. 2000 to 5000 ppm of an addition catalyst; the buffer silica gel pressure-sensitive adhesive tape prepared by the invention has better tensile viscosity loss effect, rebound resilience and buffer performance under the synergistic effect of all the components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of adhesive technology, and in particular to a stretch-debonding buffered silicone pressure-sensitive adhesive tape and a preparation method thereof. Background Art

[0002] With the development of the times, the adhesive technology has made breakthroughs step by step. Various types of adhesives can replace conventional screws or welding fixing methods, easily meeting people's bonding needs. At the same time, the softness of pressure-sensitive tape can also provide a certain buffering effect for some delicate electronic micro components or electronic product screens, camera flashes, battery packs, etc. However, after conventional pressure-sensitive tape is bonded, the adhesion is strengthened over time. Once it needs to be refurbished or replaced, the integrity of the component cannot be guaranteed.

[0003] In the prior art, there are synthetic methods using materials such as SBS, SIS, and tackifying resins to prepare stretch-debonding pressure-sensitive tapes. However, these tapes tend to become brittle and hard after aging, and bubbles are easily generated during the colloid curing process due to solvent volatilization, making it impossible for the adhesive layer to have a certain buffering capacity. Summary of the invention

[0004] In order to improve the shortcomings of traditional stretch-debonding pressure-sensitive tapes, the present application provides a stretch-debonding buffered silicone pressure-sensitive tape and a preparation method thereof.

[0005] In the first aspect, the present application provides a stretch-debonding buffered silicone pressure-sensitive adhesive tape, which adopts the following technical scheme: a stretch-debonding buffered silicone pressure-sensitive adhesive tape, comprising the following raw materials in parts by weight: 10-25 parts of spherical low-molecular methyl MQ silicone resin, 2-7 parts of terminal hydroxyl linear silicone oil, 0.01-0.03 parts of condensation catalyst, 20-35 parts of high molecular weight silicone rubber, 40-60 parts of vinyl methyl MQ silicone resin, 1-5 parts of methyl phenyl resin, 0.8-3 parts of hydrogen-containing silicone oil, 0.1-2 parts of microsphere foaming agent, 0.01-0.03 parts of inhibitor, and 2000-5000ppm of addition catalyst.

[0006] By adopting the above technical solution, the spherical low-molecular methyl MQ silicone resin is surrounded by a large number of methyl groups, and the vinyl group at the other end reacts with the hydrogen-containing silicone oil. A three-dimensional spatial structure is formed through the linking reaction of the microsphere foaming agent and the small spherical low-molecular methyl MQ silicone resin. During the stretching process, the position of the sticky group changes to achieve a change from stickiness to no stickiness, thereby achieving the effect of stretching and losing viscosity. At the same time, by introducing high-molecular silicone rubber and vinyl methyl MQ silicone resin, the pressure-sensitive adhesive tape has a certain strength structure and achieves rebound, ensuring that the viscosity of the pressure-sensitive adhesive is restored after rebound without deformation difference. Through a better spatial structure and high resilience, the pressure-sensitive adhesive can have better buffering performance. When used in some parts of electronic products, it can reduce the loss of viscosity caused by vibration and falling.

[0007] Through the coordinated cooperation of various components, the stretching length of the pressure-sensitive adhesive during the debonding process is effectively controlled, and the debonding and residual adhesive will not occur due to the bonding substrate. The addition of methylphenyl resin promotes the spatial structure to face outward, prevents oxygen attack, plays a shielding role, and ensures that the main chain is not oxidized and decomposed. It can enable the prepared pressure-sensitive adhesive to maintain good strength and bonding performance after high-temperature and long-term aging, and reduce the debonding phenomenon of conventional carbon-based colloids after aging.

[0008] Preferably, the spherical low molecular weight methyl MQ silicone resin is an oligomer of a methyl MQ silicone resin solvent; the M / Q ratio of the spherical low molecular weight methyl MQ silicone resin is 0.3-1.2, the molecular weight range of the spherical low molecular weight methyl MQ silicone resin is 400-2000, and the hydroxyl content range of the spherical low molecular weight methyl MQ silicone resin is 0.01-0.05%.

[0009] By adopting the above technical solution and selecting a low molecular weight methyl MQ silicone resin with a suitable M / Q ratio, the pressure-sensitive adhesive can maintain good adhesion and cohesion, and reduce the occurrence of cohesive failure. Selecting a molecular weight within a suitable range for the spherical methyl MQ silicone resin can keep the pressure-sensitive adhesive from being easily split internally when subjected to external forces. A molecular weight that is too large can easily lead to low surface viscosity of the pressure-sensitive adhesive and poor adhesion to the substrate surface. When the molecular weight is too small, the condensation process cannot be controlled, affecting the production of the pressure-sensitive adhesive.

[0010] Preferably, the vinyl methyl MQ silicone resin is a terminal vinyl methyl MQ silicone resin solvent, the vinyl content of the vinyl methyl MQ silicone resin is (0.02-2)%, and the molecular weight of the vinyl methyl MQ silicone resin is 3000-7000.

[0011] By adopting the above technical scheme, the vinyl groups on the end groups of the vinyl methyl MQ silicone resin and the vinyl groups on the high molecular weight silicone rubber will react with the hydrogen groups of the hydrogen-containing silicone oil. Due to the existence of steric hindrance, the vinyl groups on the end groups of the methyl MQ silicone resin will react preferentially. Therefore, selecting the vinyl content within the appropriate range of the vinyl methyl MQ silicone resin is conducive to promoting the formation of a three-dimensional structure, improving the reaction efficiency, and promoting the molded pressure-sensitive adhesive to have good strength. A high vinyl content in the vinyl methyl MQ silicone resin is likely to cause the pressure-sensitive adhesive to break easily, resulting in dead glue, and failing to achieve buffering performance. A low vinyl content is likely to fail to achieve a reinforcing effect. Therefore, controlling the vinyl content in the vinyl methyl MQ silicone resin within an appropriate range is conducive to improving the bonding strength and buffering resilience of the pressure-sensitive adhesive.

[0012] Preferably, the high molecular weight silicone rubber is a vinyl silicone rubber with a molecular weight of 60-100w and a vinyl content of 0.04-0.23%, the terminal hydroxyl content of the terminal hydroxyl linear silicone oil is (0.02-0.08) mol / 100g, and the hydrogen content of the hydrogen-containing silicone oil is 0.18-1.6%.

[0013] By adopting the above technical solution, the ethylene end of the silicone rubber reacts with the chain of the hydrogen-containing silicone oil to form a reaction structure, and the two ends of each silicone rubber long chain can link two resin macromolecules, thereby forming a stable spatial structure. When the structure changes due to external force, the movement of the resin molecules caused by the elongation direction of the silicone rubber long chain will be restricted by the movement of the resin molecules caused by the shortening direction of the silicone rubber long chain, causing the methyl convex contacts on the surface of the formed spatial structure to play a sticky role to be pulled back into the space, resulting in loss of adhesion.

[0014] Controlling the molecular weight and vinyl content of silicone rubber within an appropriate range can ensure that the pressure-sensitive adhesive remains highly viscous when it is re-laminated. If the molecular weight of silicone rubber is too high, it is easy to fail to melt during the preparation process, increasing the difficulty of production, requiring the pressure-sensitive adhesive to be stretched longer to lose its viscosity, and reducing the stretching and losing adhesion effect of the pressure-sensitive adhesive. If the molecular weight of silicone rubber is too low, it is easy to affect the strength of the pressure-sensitive adhesive, causing the pressure-sensitive adhesive to break easily.

[0015] If the terminal hydroxyl content of the hydroxyl-terminated linear silicone oil is too high, it is easy to cause the silicone oil to condense and gel. If the terminal hydroxyl content is too low, the terminal hydroxyl linear silicone oil cannot react and link with the spherical low molecular weight methyl MQ silicone resin, affecting the formation of the three-dimensional structure of the pressure-sensitive adhesive, causing the pressure-sensitive adhesive to harden and easily break. If the hydrogen content of the hydrogen-containing silicone oil is too low, it is easy to reduce the reaction efficiency and the strength of the pressure-sensitive adhesive, and if it is too high, it is easy to cause the pressure-sensitive adhesive to break easily.

[0016] Preferably, the microsphere foaming agent is at least one of yangba powder, super light clay, and paper clay.

[0017] By adopting the above technical scheme, yangbuck powder, super light clay and paper clay can be used as foaming agents to improve the flexibility of the pressure-sensitive adhesive, enhance the cushioning performance of the pressure-sensitive adhesive, absorb energy when the pressure-sensitive adhesive is impacted or vibrated, and make the pressure-sensitive adhesive less likely to break when bent or deformed.

[0018] Preferably, the condensation catalyst is at least one of sulfonic acid, ammonium chloride, barium chloride, sodium hydroxide, potassium hydroxide, sodium carbonate, tetramethylammonium hydroxide, 2,4-dichlorobenzoyl peroxide, dibenzoyl peroxide, and the like.

[0019] Preferably, the raw material of the pressure-sensitive adhesive tape further comprises 1-5 parts of cage-type polysilsesquioxane and 1-3 parts of sepiolite fiber.

[0020] By adopting the above technical solution, the silicon-hydrogen bond of the cage-type polysilsesquioxane can react with the hydroxyl group of the terminal hydroxyl linear silicone oil and the vinyl group in the silicone resin to produce chemical bonding, thereby enhancing the crosslinking degree and stability of the three-dimensional structure of the pressure-sensitive adhesive, and improving the thermal stability and tensile strength of the pressure-sensitive adhesive. Sepiolite fiber can effectively disperse stress, enhance the network structure of the pressure-sensitive adhesive, and improve the thermal stability and bonding performance of the pressure-sensitive adhesive.

[0021] Preferably, the cage-type polysilsesquioxane is an allyl cage-type polysilsesquioxane.

[0022] By adopting the above technical solution, the allyl group of cage-type polysilsesquioxane can promote the cage-type polysilsesquioxane to have higher reactivity under light, heat and chemical conditions, form a more complex network structure in the pressure-sensitive adhesive system, and improve the mechanical strength and heat aging resistance of the pressure-sensitive adhesive.

[0023] In a second aspect, the present application provides a method for preparing a stretch-debonding buffered silicone pressure-sensitive adhesive tape, using the following technical solution: A method for preparing a stretch-debonding buffered silicone pressure-sensitive adhesive tape comprises the following specific steps: Pre-mix the spherical low molecular weight methyl MQ silicone resin and the terminal hydroxyl linear silicone oil and heat them to 120-140°C, then add the condensation catalyst and continue heating the reaction for 2-3 hours to obtain product A; The vinyl methyl MQ silicone resin is heated to 90-100°C, high molecular weight silicone rubber is added and mixed, and the mixture is stirred evenly to form product B; product B and product A are heated and mixed, and the mixture is stirred evenly, and then methyl phenyl resin is added, vacuumized, cooled to 50-60°C, hydrogen-containing silicone oil, microsphere foaming agent, and inhibitor are added and mixed, and the mixture is stirred evenly, and then an addition catalyst is added to obtain a pressure-sensitive adhesive slurry, and then the pressure-sensitive slurry is scraped and coated on a release film, pressed and baked to obtain a stretch-debonding buffered silicone pressure-sensitive adhesive tape.

[0024] By adopting the above technical solution, the first step is to try to use a condensation catalyst to catalyze the reaction of spherical low-molecular methyl MQ silicone resin and terminal hydroxyl linear silicone oil, so as to fix the spherical low-molecular resin in the three-dimensional structure and reduce the loss of effective ingredients in the subsequent film forming process. At the same time, the better spatial structure of the overhead pressure-sensitive adhesive provides space for the microbubbles generated by the subsequent foaming agent to maintain the strength of the pressure-sensitive adhesive. Then, through the reaction of other components, a soft spatial structure similar to a long strip is formed, and the formed pressure-sensitive adhesive has balanced expansion and contraction, which reduces the oxidation and decomposition of the pressure-sensitive adhesive and improves the durability of the pressure-sensitive adhesive.

[0025] Preferably, the pressure-sensitive adhesive tape has a thickness of 100 μm-1000 μm.

[0026] In summary, this application has the following beneficial effects: 1. Since the present application uses spherical low molecular weight methyl MQ silicone resin, terminal hydroxyl linear silicone oil, high molecular weight silicone rubber and vinyl methyl MQ silicone resin, which react with each other to form a three-dimensional space structure, the pressure-sensitive adhesive has good stretching loss and high resilience performance, and has good buffering capacity. By introducing methyl phenyl resin, the pressure-sensitive adhesive maintains good temperature resistance and aging resistance on the basis of the original space structure.

[0027] 2. In the present application, a condensation catalyst is used to fix the spherical low-molecular resin in the three-dimensional structure, and then a soft spatial structure similar to a long strip is formed through the reaction of other components. Finally, the pressure-sensitive adhesive formed through curing has good bonding strength and stretch-loss ability. When it is laminated again, it still has high viscosity, rebounds without deformation, and has good temperature resistance and heat aging resistance. DETAILED DESCRIPTION

[0028] The present application is further described in detail below in conjunction with embodiments.

[0029] All raw materials in the examples are commercially available. Example

[0030] Example 1 The present embodiment provides a stretch-debonding buffered silicone pressure-sensitive adhesive tape, comprising the following raw materials in parts by weight: 18 kg of spherical low-molecular methyl MQ silicone resin, 4.5 kg of terminal hydroxyl linear silicone oil, 0.02 kg of condensation catalyst, 27 kg of high molecular weight silicone rubber, 50 kg of vinyl methyl MQ silicone resin, 3 kg of methyl phenyl resin, 1.9 kg of hydrogen-containing silicone oil, 1.2 kg of microsphere foaming agent, 0.02 kg of inhibitor, and 3500 ppm of addition catalyst.

[0031] The molecular weight of the spherical low molecular weight methyl MQ silicone resin is 500, the M / Q ratio of the spherical low molecular weight methyl MQ silicone resin is 0.6, and the hydroxyl content is 0.03%; the terminal hydroxyl content of the terminal hydroxyl linear silicone oil is 0.03 mol / 100 g, and the viscosity is 70 mPa.s (25°C); the molecular weight of the high molecular weight silicone rubber is 92w, the hydrogen content of the hydrogen-containing silicone oil is 1%, the vinyl methyl MQ silicone resin is a terminal vinyl methyl MQ silicone resin, the vinyl content in the vinyl methyl MQ silicone resin is 0.06%, the molecular weight of the vinyl methyl MQ silicone resin is 5000, the methyl phenyl resin is IOTA6156C type methyl phenyl silicone resin, the molecular weight is 5500, the phenyl content is 20%, the microsphere foaming agent is yangba powder, the inhibitor is methylpentynol, the catalyst is a platinum catalyst, and the condensation catalyst is ammonium chloride.

[0032] The preparation method of the stretch-debonding buffered silicone pressure-sensitive adhesive tape comprises the following specific steps: S1: Pre-dissolve the spherical low molecular weight methyl MQ silicone resin in xylene, then mix it with the terminal hydroxyl linear silicone oil, heat it to 120°C and keep it for 1 hour, then add one third of the condensation catalyst and continue to heat it to 135°C, stir and react at a constant temperature for 2.5 hours, then add the remaining condensation catalyst to obtain product A.

[0033] S2: Dissolve vinyl methyl MQ silicone resin in xylene, mix with high molecular weight silicone rubber, heat and dissolve with stirring for 2 hours to obtain product B.

[0034] S3: Heat product B to 125°C and add product A, stir for 30 minutes, dissolve methylphenyl resin in xylene and add it to product B, vacuum degassing, cool to 55°C, add hydrogenated silicone oil, microsphere foaming agent and inhibitor, mix, stir for 30 minutes, filter and obtain semi-finished product C, then mix semi-finished product C with catalyst, apply it on release film through double-blade slit scraper coater, adjust the average thickness to 500μm, press and bake at 140°C for 3 minutes, and obtain buffered silicone pressure-sensitive tape after die-cutting.

[0035] Example 2 The difference between Example 2 and Example 1 is that the amount of spherical low-molecular methyl MQ silicone resin used in the buffer silicone pressure-sensitive tape raw material is 10 kg, the amount of terminal hydroxyl linear silicone oil used is 7 kg, the amount of condensation catalyst used is 0.01 kg, the amount of high molecular weight silicone rubber used is 20 kg, the amount of vinyl methyl MQ silicone resin used is 60 kg, the amount of methyl phenyl resin used is 5 kg, the amount of hydrogen-containing silicone oil used is 0.8 kg, the amount of microsphere foaming agent used is 0.1 kg, the amount of inhibitor used is 0.03 kg, and the amount of addition catalyst used is 2000 ppm.

[0036] Example 3 The difference between Example 3 and Example 1 is that the amount of spherical low-molecular methyl MQ silicone resin used in the buffer silicone pressure-sensitive tape raw material is 25kg, the amount of terminal hydroxyl linear silicone oil used is 2kg, the amount of condensation catalyst used is 0.03kg, the amount of high molecular weight silicone rubber used is 35kg, the amount of vinyl methyl MQ silicone resin used is 40kg, the amount of methyl phenyl resin used is 1kg, the amount of hydrogen-containing silicone oil used is kg, the amount of microsphere foaming agent used is 2kg, the amount of inhibitor used is 0.01kg, and the amount of addition catalyst used is 5000ppm.

[0037] Example 4 The difference between Example 4 and Example 1 is that the molecular weight of the spherical low molecular weight methyl MQ silicone resin in the raw material of the buffer silicone pressure-sensitive adhesive tape is 2000.

[0038] Example 5 The difference between Example 5 and Example 1 is that the terminal hydroxyl content of the terminal hydroxyl linear silicone oil in the buffer silicone pressure-sensitive adhesive tape raw material is 0.08 mol / 100 g.

[0039] Example 6 The difference between Example 6 and Example 1 is that the molecular weight of the high molecular weight silicone rubber in the raw material of the buffer silicone pressure-sensitive adhesive tape is 100w.

[0040] Example 7 The difference between Example 7 and Example 1 is that the vinyl content in the vinyl methyl MQ silicone resin in the raw material of the buffer silicone pressure-sensitive adhesive tape is 3%.

[0041] Example 8 The difference between Example 8 and Example 1 is that in the preparation method of the buffered silicone pressure-sensitive adhesive tape, the reaction time of the product A is different.

[0042] The preparation method of the stretch-debonding buffered silicone pressure-sensitive adhesive tape comprises the following specific steps: S1: Dissolve the spherical low molecular weight methyl MQ silicone resin in xylene in advance, then mix it with the terminal hydroxyl linear silicone oil, heat it to 120°C and keep it for 1 hour, then add one third of the condensation catalyst and continue to heat it to 135°C, stir and react at a constant temperature for 4 hours, then add the remaining condensation catalyst to obtain product A.

[0043] S2: Dissolve vinyl methyl MQ silicone resin in xylene, mix with high molecular weight silicone rubber, heat and dissolve with stirring for 2 hours to obtain product B.

[0044] S3: Heat product B to 125°C and add product A, stir for 30 minutes, dissolve methylphenyl resin in xylene and add it to product B, vacuum degassing, cool to 55°C, add hydrogenated silicone oil, microsphere foaming agent and inhibitor, mix, stir for 30 minutes, filter and obtain semi-finished product C, then mix semi-finished product C with catalyst, apply it on release film through double-blade slit scraper coater, adjust the average thickness to 500μm, press and bake at 140°C for 3 minutes, and obtain buffered silicone pressure-sensitive tape after die-cutting.

[0045] Example 9 The difference between Example 9 and Example 1 is that the raw material of the buffer silicone pressure-sensitive adhesive tape further includes 3 kg of cage-type polysilsesquioxane, which is POSS-JH-2P2016.

[0046] The preparation method of the stretch-debonding buffered silicone pressure-sensitive adhesive tape comprises the following specific steps: S1: Pre-dissolve the spherical low molecular weight methyl MQ silicone resin in xylene, then mix it with the terminal hydroxyl linear silicone oil, heat it to 120°C and keep it for 1 hour, then add one third of the condensation catalyst and continue to heat it to 135°C, stir and react at a constant temperature for 2.5 hours, then add the remaining condensation catalyst to obtain product A.

[0047] S2: Dissolve vinyl methyl MQ silicone resin in xylene, mix with high molecular weight silicone rubber, heat and dissolve with stirring for 2 hours to obtain product B.

[0048] S3: Heat product B to 125°C and add product A, stir for 30 minutes, dissolve methylphenyl resin in xylene and add it to product B, vacuum degassing, cool to 55°C, add cage-type polysilsesquioxane, hydrogenated silicone oil, microsphere foaming agent, and inhibitor, mix, stir for 30 minutes, filter the material to obtain semi-finished product C, then mix the semi-finished product C with the catalyst, apply it on the release film through a double-blade slit scraper coater, adjust the average thickness to 500 μm, press and bake at 140°C for 3 minutes, and obtain the buffered silicone pressure-sensitive tape after die-cutting.

[0049] Example 10 The difference between Example 10 and Example 9 is that the raw material of the buffer silicone pressure-sensitive adhesive tape further includes 2 kg of sepiolite fiber.

[0050] The preparation method of the stretch-debonding buffered silicone pressure-sensitive adhesive tape comprises the following specific steps: S1: Pre-dissolve the spherical low molecular weight methyl MQ silicone resin in xylene, then mix it with the terminal hydroxyl linear silicone oil, heat it to 120°C and keep it for 1 hour, then add one third of the condensation catalyst and continue to heat it to 135°C, stir and react at a constant temperature for 2.5 hours, then add the remaining condensation catalyst to obtain product A.

[0051] S2: Dissolve vinyl methyl MQ silicone resin in xylene, mix with high molecular weight silicone rubber, heat and dissolve with stirring for 2 hours to obtain product B.

[0052] S3: Heat product B to 125°C and add product A, stir for 30 minutes, dissolve methylphenyl resin in xylene and add it to product B, vacuum degassing, cool to 55°C, add cage-type polysilsesquioxane, sepiolite fiber, hydrogenated silicone oil, microsphere foaming agent, and inhibitor, mix, stir for 30 minutes, filter the material to obtain semi-finished product C, then mix the semi-finished product C with the catalyst, apply it on the release film through a double-blade slit scraper coater, adjust the average thickness to 500 μm, press and bake at 140°C for 3 minutes, and obtain the buffered silicone pressure-sensitive tape after die-cutting.

[0053] Embodiment 11 The difference between Example 11 and Example 10 is that the amount of sepiolite fiber used in the raw material of the buffer silicone pressure-sensitive adhesive tape is 3 kg, and the amount of cage-type polysilsesquioxane used is 1 kg.

[0054] Example 12 The difference between Example 12 and Example 10 is that the amount of sepiolite fiber used in the raw material of the buffer silicone pressure-sensitive adhesive tape is 1 kg, and the amount of cage-type polysilsesquioxane used is 5 kg.

[0055] Example 13 The difference between Example 13 and Example 10 is that an equal amount of allyl cage polysilsesquioxane is used in the raw material of the buffered silicone pressure-sensitive adhesive tape instead of cage polysilsesquioxane. Allyl cage polysilsesquioxane is selected from Guangdong Wengjiang Reagent Co., Ltd., CAS No. 1620202-27-8, and the molecular weight is 1192.0.

[0056] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that no methyl phenyl resin is used in the raw material of the buffer silicone pressure-sensitive adhesive tape.

[0057] Performance testing The following performance tests were performed on the buffered silicone pressure-sensitive adhesive tapes provided in Examples 1-13 of the present application and Comparative Example 1. The specific test results are shown in Table 1.

[0058] Detection Methods 1. Viscosity test With reference to the standard of GB / T 2792-2014 "Test method for 180° peel strength of adhesive tape", the viscosity of the stretch-debonding buffered silicone pressure-sensitive tape prepared in this application was tested, and the elongation of the pressure-sensitive tape was manually measured when the viscosity of the pressure-sensitive tape decreased by 50% and 100%.

[0059] 2. Point impact absorption rate The impact force absorption ratio of the stretch-debonding buffer silicone pressure-sensitive adhesive tape prepared in the present application was tested in the vertical direction using a foam cushioning performance impact strength tester.

[0060] 3. Hardness test After baking at a high temperature of 260° C. for 7 days, the appearance of the pressure-sensitive tape was observed, and the Shore A hardness of the stretch-debonding buffered silicone pressure-sensitive tape prepared in the present application was tested using a Shore A durometer.

[0061] Table 1: Performance test results data table It can be seen from the performance test results that the pressure-sensitive adhesive tape prepared by the present application has good bonding performance, resilience and buffering performance under the synergistic effect of each component, and the impact absorption rate of the pressure-sensitive adhesive test point can reach more than 94%, which further proves that the pressure-sensitive adhesive can absorb most of the instantaneous stress, thereby protecting the substrate bonded by the pressure-sensitive adhesive tape and reducing the adverse phenomenon caused by the substrate falling due to vibration. At the same time, the pressure-sensitive adhesive tape prepared by the present application has good thermal stability and aging resistance. After baking at high temperature for one week, it still maintains good bonding and buffering performance, can maintain good elongation loss and viscosity recovery after unloading, and has no residual glue, precipitation, and cracking. By comparing Comparative Example 1 with Example 1, it can be seen that if methylphenyl resin is not used in the pressure-sensitive adhesive raw material, it is easy to cause the thermal stability and strength of the pressure-sensitive adhesive to be significantly reduced, thereby reducing the tensile loss and resilience of the pressure-sensitive adhesive.

[0062] By comparing Example 4 with Example 1, it can be seen that if the molecular weight of the spherical low molecular weight methyl MQ silicone resin is too high, it is easy to reduce the surface viscosity of the pressure-sensitive adhesive, thereby affecting the adhesive performance of the pressure-sensitive adhesive. Therefore, selecting the molecular weight of the spherical low molecular weight methyl MQ silicone resin within the appropriate molecular weight range is also crucial to the performance of the pressure-sensitive adhesive.

[0063] By comparing Example 5 with Example 1, it can be seen that the terminal hydroxyl content of the terminal hydroxyl linear silicone oil is too high. Although the pressure-sensitive adhesive still maintains good comprehensive performance, the silicone oil in the pressure-sensitive adhesive raw material undergoes self-condensation during the reaction, which is also likely to affect the tensile loss properties of the pressure-sensitive adhesive.

[0064] By comparing Example 6 with Example 1, it can be seen that the high molecular weight silicone rubber has a too high molecular weight, which easily causes the phenomenon of not being able to melt when hot-melted. The pressure-sensitive adhesive needs to be stretched longer to lose its viscosity, resulting in a reduction in the stretching and debonding effect of the pressure-sensitive adhesive.

[0065] By comparing Example 7 with Example 1, it can be seen that the vinyl content in the vinyl methyl MQ silicone resin is likely to affect the strength of the pressure-sensitive adhesive. Too high a vinyl content is likely to cause dead glue and reduce the buffering performance. Too low a vinyl content will not play a reinforcing role.

[0066] By comparing Example 8 with Example 1, it can be seen that changing the reaction time of Product 1 will also affect the comprehensive performance of the pressure-sensitive adhesive. Too long a time may easily cause the pressure-sensitive adhesive to be too sticky, while too short a time may easily cause an incomplete reaction, thereby affecting the bonding performance of the pressure-sensitive adhesive.

[0067] By comparing Examples 9-13 with Example 1, it can be seen that cage-type polysilsesquioxane and sepiolite fiber have a significant promoting effect on the thermal stability, bonding strength and tensile loss properties of the pressure-sensitive adhesive. At the same time, allyl cage-type polysilsesquioxane can have a higher reaction efficiency with other components in the pressure-sensitive adhesive raw material, further improving the comprehensive performance of the pressure-sensitive adhesive.

[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A stretch-debonding buffered silicone pressure-sensitive adhesive tape, characterized in that: The invention comprises the following raw materials in parts by weight: 10-25 parts of spherical low molecular weight methyl MQ silicone resin, 2-7 parts of terminal hydroxyl linear silicone oil, 0.01-0.03 parts of condensation catalyst, 20-35 parts of high molecular weight silicone rubber, 40-60 parts of vinyl methyl MQ silicone resin, 1-5 parts of methyl phenyl resin, 0.8-3 parts of hydrogen-containing silicone oil, 0.1-2 parts of microsphere foaming agent, 0.01-0.03 parts of inhibitor and 2000-5000ppm of addition catalyst.

2. The stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 1, characterized in that: The spherical low molecular weight methyl MQ silicone resin is an oligomer of a methyl MQ silicone resin solvent; the M / Q ratio of the spherical low molecular weight methyl MQ silicone resin is 0.3-1.2, the molecular weight of the spherical low molecular weight methyl MQ silicone resin is in the range of 400-2000, and the hydroxyl content of the spherical low molecular weight methyl MQ silicone resin is in the range of 0.01-0.05%.

3. The stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 1, characterized in that: The vinyl methyl MQ silicone resin is a terminal vinyl methyl MQ silicone resin solvent, the vinyl content of the vinyl methyl MQ silicone resin is (0.02-2)%, and the molecular weight of the vinyl methyl MQ silicone resin is 3000-7000.

4. The stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 1, characterized in that: The high molecular weight silicone rubber is a vinyl silicone rubber with a molecular weight of 60-100w and a vinyl content of 0.04-0.23%. The terminal hydroxyl content of the terminal hydroxyl linear silicone oil is (0.02-0.08) mol / 100g. The hydrogen content of the hydrogen-containing silicone oil is 0.18-1.6%.

5. The stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 1, characterized in that: The microsphere foaming agent is at least one of yangba powder, super light clay and paper clay.

6. The stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 1, characterized in that: The condensation catalyst is at least one of sulfonic acid, ammonium chloride, barium chloride, sodium hydroxide, potassium hydroxide, sodium carbonate, tetramethylammonium hydroxide, 2,4-dichlorobenzoyl peroxide, dibenzoyl peroxide, and the like.

7. The stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 1, characterized in that: The raw materials of the pressure-sensitive adhesive tape also include 1-5 parts of cage-type polysilsesquioxane and 1-3 parts of sepiolite fibers.

8. The stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 7, characterized in that: The cage-type polysilsesquioxane is allyl cage-type polysilsesquioxane.

9. A method for preparing a stretch-debonding buffered silicone pressure-sensitive adhesive tape according to any one of claims 1 to 8, characterized in that: The specific steps include: Pre-mix the spherical low molecular weight methyl MQ silicone resin and the terminal hydroxyl linear silicone oil and heat them to 120-140°C, then add the condensation catalyst and continue heating the reaction for 2-3 hours to obtain product A; Heat the vinyl methyl MQ silicone resin to 90-100°C, add the high molecular weight silicone rubber and mix, and stir evenly to form product B; Heat and mix product B and product A, stir evenly, then add methylphenyl resin, evacuate, cool to 50-60°C, add hydrogenated silicone oil, microsphere foaming agent, inhibitor, mix, stir evenly, then add addition catalyst to obtain pressure-sensitive adhesive slurry, then scrape the pressure-sensitive slurry on the release film, press and bake to obtain stretch-debonding buffered silicone pressure-sensitive tape.

10. The method for preparing the stretch-debonding buffered silicone pressure-sensitive adhesive tape according to claim 9, characterized in that: The thickness of the pressure-sensitive adhesive tape is 100 μm-1000 μm.

Citation Information

Patent Citations

  • Easy-to-pull removable adhesive tape

    CN110669451A

  • High-temperature-resistant stable organic silicon pressure-sensitive adhesive as well as preparation method and application thereof

    CN116904158A

  • Safe explosion-proof easy-to-disassemble adhesive tape and preparation method therefor

    WO2018129899A1