High-strength high-temperature-resistant binder

By combining modified epoxy resin and reinforced components, the heat resistance and bonding strength of the adhesive are improved, and the shortcomings of existing adhesives in high temperature resistance and bonding effects are solved, thus achieving higher Bonding strength and heat resistance.

CN118931447APending Publication Date: 2024-11-12SHANGHAI CARBON BEAM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411144893.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The bonding effect of existing adhesives is not high in some application scenarios, and their high temperature resistance and overall bonding strength need to be improved.

Method used

Using modified epoxy resin, reinforced curing agent, filler, fiber and whisker, the heat resistance and toughness of the adhesive are improved through specific preparation steps and process processing, and the cracks of the adhesive layer are prevented from spreading, thereby enhancing the Bonding strength.

Benefits of technology

It effectively improves the overall heat resistance and bonding strength of the adhesive, enhances the overall performance of the adhesive, and solves the shortcomings of bonding effect and high temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001938710000071
    Figure BDA0005001938710000071
  • Figure BDA0005001938710000082
    Figure BDA0005001938710000082
Patent Text Reader

Abstract

The invention discloses a high-strength high-temperature-resistant binder, and relates to the technical field of high-temperature-resistant binders. The high-strength and high-temperature-resistant binder is prepared from the following components in parts by mass: 20 to 35 parts of modified epoxy resin, 20 to 35 parts of diallyl bisphenol, 10 to 20 parts of diphenylmethane bismaleimide resin, 5 to 8 parts of a reinforcing component and 1 to 2 parts of an auxiliary agent, the reinforcing component comprises 1-3 parts of a reinforcing curing agent, 1-2 parts of a reinforcing filler, 0.5-1 part of reinforcing fibers and 1-2 parts of reinforcing whiskers; the preparation raw material of the adhesive is replaced by the modified epoxy resin, the heat resistance and toughness of the epoxy resin can be effectively improved due to high bond energy of Si-O in organic silicon, the overall heat resistance and bonding strength of the adhesive can be further improved, and meanwhile, the reinforcing component is added in the preparation process, so that the bonding strength of the adhesive is improved, and the service life of the adhesive is prolonged. Further, crack propagation of the adhesive layer can be prevented, and the overall bonding strength of the adhesive is further enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high temperature resistant adhesives, and in particular relates to a high strength high temperature resistant adhesive. Background Art

[0002] Bonding is a method of firmly connecting the same or different materials together through substances with adhesion ability. Substances with adhesion ability are called adhesives. The bonding process is a complex physical and chemical process. The quality of bonding performance not only depends on the structure and state of the adhesive and the surface of the adherend, but is also closely related to the process conditions of the bonding process. In industrial production, adhesives play a very important role. They are widely used in construction, automobile manufacturing, aerospace, electronic equipment, casting production and other fields. However, traditional adhesives have some disadvantages in some specific application scenarios, such as low bonding strength, poor heat resistance, poor environmental friendliness and other problems.

[0003] Existing patent CN102115653B discloses a binder composition, which includes two components A and B; component A is obtained by reacting epoxy resin and / or phenolic resin, chloroprene rubber, glass fiber, inorganic nanomaterial, complexing agent and silane coupling agent at 120-150°C for 70-90 minutes; wherein the inorganic nanomaterial is a mixture of calcium fluoride and at least one of silicon oxide, manganese oxide, aluminum oxide and titanium oxide. The binder composition in this patent document can bond two different metals. The existing patent CN106519992A provides an adhesive, including the following components: 30-90 parts by weight of ceramic powder, 10-50 parts by weight of organic resin, 0.1-5 parts by weight of auxiliary agent, 5-10 parts by weight of filler, and 10-50 parts by weight of organic solvent; wherein: the ceramic powder is oxide ceramic powder, nitride ceramic powder, carbide ceramic powder or boride ceramic powder, the particle size of the ceramic powder is 1-5μm, the organic resin is acrylate, polyurethane, silicone resin or epoxy resin, the auxiliary agent is a curing agent, a dispersant and a defoaming agent, and the filler is one or more of CaCO3, CaO and SiO2. By using the ceramic powder as a matrix and the organic resin as an adhesive carrier for bonding, a composite material with excellent pressure resistance and thermal conductivity can be obtained.

[0004] However, the adhesives in the prior art still have certain deficiencies. The bonding effect of the adhesives in the above scheme may not be high, and the high temperature resistance and overall bonding strength need to be further improved. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a high-strength, high-temperature resistant adhesive that can overcome the above problems or at least partially solve the above problems.

[0006] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is: a high-strength and high-temperature resistant adhesive, comprising the following components in parts by mass:

[0007] 20-35 parts of modified epoxy resin, 20-35 parts of diallyl bisphenol, 10-20 parts of diphenylmethane bismaleimide resin, 5-8 parts of reinforcing component, 1-2 parts of auxiliary agent;

[0008] The reinforcing components include 1-3 parts of reinforcing curing agent, 1-2 parts of reinforcing filler, 0.5-1 parts of reinforcing fiber, and 1-2 parts of reinforcing whisker.

[0009] Furthermore, the modified epoxy resin comprises the following components in parts by mass: 30-40 parts of epoxy resin, 30-40 parts of silicone resin, 5-10 parts of silicone oil, and 5-10 parts of organosilicon;

[0010] The specific preparation steps of the modified epoxy resin are as follows:

[0011] Step 1: Put epoxy resin and silicone resin into a reactor and heat to 90-100°C;

[0012] Step 2: crush and sieve the organosilicon, add the sieved organosilicon into the reactor, and heat to 110-130° C. for reaction;

[0013] Step 3: Add silicone oil into the reactor and stir thoroughly for 40-50 minutes to obtain a mixed solution;

[0014] Step 4: dehydrate the mixed solution by atmospheric distillation and filter to obtain the modified epoxy resin.

[0015] Preferably, the reinforcing curing agent is one or more of m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone and methylhexahydrophthalic anhydride.

[0016] Furthermore, the reinforcing filler is any one of calcium carbonate, iron powder, silicon powder and carbon black.

[0017] Furthermore, the reinforcing fiber is one or more of glass fiber, vinylon fiber, polyvinyl alcohol fiber and polyphenylene sulfide fiber.

[0018] Furthermore, the reinforcing whiskers are one or more of zinc oxide whiskers, calcium sulfate whiskers, calcium carbonate whiskers, aluminum borate whiskers, titanium-based whiskers, hydroxyapatite whiskers, magnesium hydroxide whiskers, basic magnesium sulfate whiskers and silicon carbide whiskers.

[0019] Preferably, the auxiliary agent is a mixture of an antioxidant, a stabilizer, a toughening agent and a coupling agent.

[0020] Furthermore, the mass ratio of the antioxidant, stabilizer, toughening agent and coupling agent is 1:1:2:5.

[0021] Furthermore, the diameter of the reinforced whisker is 50-70 μm, and the length of the reinforced whisker is 500-600 μm.

[0022] Furthermore, in the step 2, when the organosilicon is crushed and sieved, the mesh size of the sieve is 2500-3000 mesh.

[0023] After adopting the above technical scheme, the present invention has the following beneficial effects compared with the prior art: the present invention replaces the raw materials for preparing the adhesive with modified epoxy resin, and through the high Si-O bond energy in silicone, it can effectively improve the heat resistance and toughness of the epoxy resin, thereby improving the overall heat resistance and bonding strength of the adhesive, and at the same time, by adding reinforcing components during the preparation process, it can prevent crack propagation in the adhesive layer, thereby further enhancing the overall bonding strength of the adhesive. DETAILED DESCRIPTION

[0024] Embodiment 1:

[0025] A high-strength and high-temperature resistant adhesive, comprising the following components in parts by weight:

[0026] 28 parts of modified epoxy resin, 28 parts of diallyl bisphenol, 15 parts of diphenylmethane bismaleimide resin, 6 parts of reinforcing component, 1 part of auxiliary agent;

[0027] The reinforcing component comprises 2 parts of reinforcing curing agent, 2 parts of reinforcing filler, 0.8 parts of reinforcing fiber and 1 part of reinforcing whisker.

[0028] The modified epoxy resin comprises the following components in parts by mass: 35 parts of epoxy resin, 35 parts of silicone resin, 8 parts of silicone oil, and 8 parts of organic silicon;

[0029] The specific preparation steps of the modified epoxy resin are as follows:

[0030] Step 1: Put epoxy resin and silicone resin into a reactor and heat to 95°C;

[0031] Step 2: crush and sieve the organosilicon, add the sieved organosilicon into the reactor, and heat to 120° C. for reaction;

[0032] Step 3: Add silicone oil into the reactor and stir thoroughly for 45 minutes to obtain a mixed solution;

[0033] Step 4: dehydrate the mixed solution by atmospheric distillation and filter to obtain the modified epoxy resin.

[0034] The reinforcing curing agent is m-phenylenediamine.

[0035] The reinforcing filler is calcium carbonate.

[0036] The reinforcing fiber is glass fiber.

[0037] The reinforcing whiskers are zinc oxide whiskers.

[0038] The auxiliary agent is a mixture of an antioxidant, a stabilizer, a toughening agent and a coupling agent.

[0039] The mass ratio of the antioxidant, stabilizer, toughening agent and coupling agent is 1:1:2:5.

[0040] The diameter of the reinforced whisker is 60 μm, and the length of the reinforced whisker is 550 μm.

[0041] When the organosilicon is crushed and sieved in the step 2, the mesh number of the sieve is 2800 meshes.

[0042] Embodiment 2:

[0043] A high-strength and high-temperature resistant adhesive, comprising the following components in parts by weight:

[0044] 28 parts of modified epoxy resin, 28 parts of diallyl bisphenol, 15 parts of diphenylmethane bismaleimide resin, 6 parts of reinforcing component, 1 part of auxiliary agent;

[0045] The reinforcing component comprises 2 parts of reinforcing curing agent, 2 parts of reinforcing filler, 0.8 parts of reinforcing fiber and 1 part of reinforcing whisker.

[0046] The modified epoxy resin comprises the following components in parts by mass: 35 parts of epoxy resin, 35 parts of silicone resin, 8 parts of silicone oil, and 8 parts of organic silicon;

[0047] The specific preparation steps of the modified epoxy resin are as follows:

[0048] Step 1: Put epoxy resin and silicone resin into a reactor and heat to 95°C;

[0049] Step 2: crush and sieve the organosilicon, add the sieved organosilicon into the reactor, and heat to 120° C. for reaction;

[0050] Step 3: Add silicone oil into the reactor and stir thoroughly for 45 minutes to obtain a mixed solution;

[0051] Step 4: dehydrate the mixed solution by atmospheric distillation and filter to obtain the modified epoxy resin.

[0052] The reinforcing curing agent is m-phenylenediamine and diaminodiphenylmethane.

[0053] The reinforcing filler is calcium carbonate.

[0054] The reinforcing fibers are glass fibers, vinylon fibers and polyvinyl alcohol fibers.

[0055] The reinforcing whiskers are zinc oxide whiskers, calcium sulfate whiskers, calcium carbonate whiskers and aluminum borate whiskers.

[0056] The auxiliary agent is a mixture of an antioxidant, a stabilizer, a toughening agent and a coupling agent.

[0057] The mass ratio of the antioxidant, stabilizer, toughening agent and coupling agent is 1:1:2:5.

[0058] The diameter of the reinforced whisker is 60 μm, and the length of the reinforced whisker is 550 μm.

[0059] When the organosilicon is crushed and sieved in the step 2, the mesh number of the sieve is 2800 meshes.

[0060] Embodiment 3:

[0061] A high-strength and high-temperature resistant adhesive, comprising the following components in parts by weight:

[0062] 30 parts of modified epoxy resin, 30 parts of diallyl bisphenol, 18 parts of diphenylmethane bismaleimide resin, 8 parts of reinforcing component, 2 parts of auxiliary agent;

[0063] The reinforcing component comprises 2 parts of reinforcing curing agent, 1 part of reinforcing filler, 1 part of reinforcing fiber and 2 parts of reinforcing whisker.

[0064] The modified epoxy resin comprises the following components in parts by weight: 40 parts of epoxy resin, 40 parts of silicone resin, 10 parts of silicone oil, and 10 parts of organic silicon;

[0065] The specific preparation steps of the modified epoxy resin are as follows:

[0066] Step 1: Put epoxy resin and silicone resin into a reactor and heat to 95°C;

[0067] Step 2: crush and sieve the organosilicon, add the sieved organosilicon into the reactor, and heat to 120° C. for reaction;

[0068] Step 3: Add silicone oil into the reactor and stir thoroughly for 45 minutes to obtain a mixed solution;

[0069] Step 4: dehydrate the mixed solution by atmospheric distillation and filter to obtain the modified epoxy resin.

[0070] The reinforcing curing agent is m-phenylenediamine.

[0071] The reinforcing filler is calcium carbonate.

[0072] The reinforcing fiber is glass fiber.

[0073] The reinforcing whiskers are zinc oxide whiskers.

[0074] The auxiliary agent is a mixture of an antioxidant, a stabilizer, a toughening agent and a coupling agent.

[0075] The mass ratio of the antioxidant, stabilizer, toughening agent and coupling agent is 1:1:2:5.

[0076] The diameter of the reinforced whisker is 60 μm, and the length of the reinforced whisker is 550 μm.

[0077] When the organosilicon is crushed and sieved in the step 2, the mesh number of the sieve is 2800 meshes.

[0078] Embodiment 4:

[0079] A high-strength and high-temperature resistant adhesive, comprising the following components in parts by weight:

[0080] 28 parts of modified epoxy resin, 28 parts of diallyl bisphenol, 15 parts of diphenylmethane bismaleimide resin, 6 parts of reinforcing component, 1 part of auxiliary agent;

[0081] The reinforcing component comprises 2 parts of reinforcing curing agent, 2 parts of reinforcing filler, 0.8 parts of reinforcing fiber and 1 part of reinforcing whisker.

[0082] The modified epoxy resin comprises the following components in parts by mass: 35 parts of epoxy resin, 35 parts of silicone resin, 8 parts of silicone oil, and 8 parts of organic silicon;

[0083] The specific preparation steps of the modified epoxy resin are as follows:

[0084] Step 1: Put epoxy resin and silicone resin into a reactor and heat to 95°C;

[0085] Step 2: crush and sieve the organosilicon, add the sieved organosilicon into the reactor, and heat to 120° C. for reaction;

[0086] Step 3: Add silicone oil into the reactor and stir thoroughly for 45 minutes to obtain a mixed solution;

[0087] Step 4: dehydrate the mixed solution by atmospheric distillation and filter to obtain the modified epoxy resin.

[0088] The reinforcing curing agent is m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone and methylhexahydrophthalic anhydride.

[0089] The reinforcing fillers are calcium carbonate, iron powder, silicon powder and carbon black.

[0090] The reinforcing fibers are glass fibers, vinylon fibers, polyvinyl alcohol fibers and polyphenylene sulfide fibers.

[0091] The reinforcing whiskers are zinc oxide whiskers, calcium sulfate whiskers, calcium carbonate whiskers, aluminum borate whiskers, titanium-based whiskers, hydroxyapatite whiskers, magnesium hydroxide whiskers, basic magnesium sulfate whiskers and silicon carbide whiskers.

[0092] The auxiliary agent is a mixture of an antioxidant, a stabilizer, a toughening agent and a coupling agent.

[0093] The mass ratio of the antioxidant, stabilizer, toughening agent and coupling agent is 1:1:2:5.

[0094] The diameter of the reinforced whisker is 60 μm, and the length of the reinforced whisker is 550 μm.

[0095] When the organosilicon is crushed and sieved in the step 2, the mesh number of the sieve is 2800 meshes.

[0096] Comparative Example 1:

[0097] A high-strength and high-temperature resistant adhesive is basically the same as Example 1, except that the adhesive is composed of 28 parts of epoxy resin, 28 parts of diallyl bisphenol, 15 parts of diphenylmethane bismaleimide resin, 6 parts of reinforcing component, and 1 part of auxiliary agent.

[0098] Comparative Example 2:

[0099] A high-strength and high-temperature resistant adhesive is basically the same as Example 1, except that the adhesive is composed of 28 parts of modified epoxy resin, 28 parts of diallyl bisphenol, 15 parts of diphenylmethane bismaleimide resin, and 1 part of an auxiliary agent.

[0100] In combination with Example 1 to Example 4 and Comparative Example 1 to Comparative Example 2, the adhesives prepared in each group of Examples and Comparative Examples were tested, and the specific experimental steps are as follows:

[0101] Take the adhesives in each group of embodiments and comparative examples, and divide the adhesives obtained in each group into 10 cases, evenly apply each case of adhesive on a test plate of the same size and material, and cover and bond the same test plates accordingly, and perform a tensile test after cooling and placing (it should be noted that the test data is the average value of the comprehensive data of 10 cases). Specific test data are shown in Table 1:

[0102]

[0103]

[0104] Table 1

[0105] Then take each adhesive and evenly apply it on the test plates of the same size and material, and cover and bond the same test plates together. After heating, observe the tensile strength of each group of adhesives. The specific data are shown in Table 2:

[0106]

[0107] Table 2

[0108] In summary, referring to Table 1, Table 2 and Example 4, the present invention replaces the raw materials for preparing the adhesive with modified epoxy resin, and through the high bond energy of Si-O in silicone, it can effectively improve the heat resistance and toughness of the epoxy resin, thereby improving the overall heat resistance and bonding strength of the adhesive, and at the same time, by adding reinforcing components during the preparation process, it can prevent crack propagation in the adhesive layer, thereby further enhancing the overall bonding strength of the adhesive.

[0109] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.

Claims

1. A high-strength and high-temperature resistant adhesive, It is characterized in that The composition includes the following components by mass: 20-35 parts of modified epoxy resin, 20-35 parts of diallyl bisphenol, 10-20 parts of diphenylmethane bismaleimide resin, 5-8 parts of reinforcing component, 1-2 parts of auxiliary agent; The reinforcing components include 1-3 parts of reinforcing curing agent, 1-2 parts of reinforcing filler, 0.5-1 parts of reinforcing fiber, and 1-2 parts of reinforcing whisker.

2. A high-strength and high-temperature resistant adhesive according to claim 1, It is characterized in that The modified epoxy resin comprises the following components in parts by weight: 30-40 parts of epoxy resin, 30-40 parts of silicone resin, 5-10 parts of silicone oil, and 5-10 parts of organic silicon; The specific preparation steps of the modified epoxy resin are as follows: Step 1: Put epoxy resin and silicone resin into a reactor and heat to 90-100°C; Step 2: crush and sieve the organosilicon, add the sieved organosilicon into the reactor, and heat to 110-130° C. for reaction; Step 3: Add silicone oil into the reactor and stir thoroughly for 40-50 minutes to obtain a mixed solution; Step 4: dehydrate the mixed solution by atmospheric distillation and filter to obtain the modified epoxy resin.

3. A high-strength and high-temperature resistant adhesive according to claim 1, It is characterized in that The reinforcing curing agent is one or more of m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone and methylhexahydrophthalic anhydride.

4. A high-strength and high-temperature resistant adhesive according to claim 3, It is characterized in that The reinforcing filler is any one of calcium carbonate, iron powder, silicon powder and carbon black.

5. A high-strength and high-temperature resistant adhesive according to claim 3, It is characterized in that The reinforcing fiber is one or more of glass fiber, vinylon fiber, polyvinyl alcohol fiber and polyphenylene sulfide fiber.

6. A high-strength and high-temperature resistant adhesive according to claim 3, It is characterized in that The reinforcing whiskers are one or more of zinc oxide whiskers, calcium sulfate whiskers, calcium carbonate whiskers, aluminum borate whiskers, titanium-based whiskers, hydroxyapatite whiskers, magnesium hydroxide whiskers, basic magnesium sulfate whiskers and silicon carbide whiskers.

7. A high-strength and high-temperature resistant adhesive according to claim 1, It is characterized in that The auxiliary agent is a mixture of an antioxidant, a stabilizer, a toughening agent and a coupling agent.

8. A high-strength and high-temperature resistant adhesive according to claim 7, It is characterized in that The mass ratio of the antioxidant, stabilizer, toughening agent and coupling agent is 1:1:2:

5.

9. A high-strength and high-temperature resistant adhesive according to claim 3, It is characterized in that The diameter of the reinforced whisker is 50-70 μm, and the length of the reinforced whisker is 500-600 μm.

10. A high-strength and high-temperature resistant adhesive according to claim 2, It is characterized in that When the organosilicon is crushed and sieved in the step 2, the mesh size of the sieve is 2500-3000 mesh.